CuZn40 (C28000) Muntz Metal, Hard Material Data Sheet

CuZn40 (C28000) Muntz Metal Material Data Sheet (Wrought, Hard)

CuZn40 C28000 Hard Overview

CuZn40 C28000 hard is a wrought brass (UNS C28000), known as muntz metal. Condition: Hard. This CuZn40 C28000 hard material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn40 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn40 brass parts in-house and inspects them before shipment.

CuZn40 Designation

CuZn40, wrought
ConditionHard
UNS numberC28000
EN nameCW509L
ISO nameCuZn40
JIS (Japanese) nameC2800 / C2801

CuZn40 Typical uses

Hot-formed parts, extruded sections, forgings, condenser plates.

CuZn40 C28000 Hard Composition detail

Cu (copper)58.6–63.4%
Fe (iron)0–0.07%
Pb (lead)0–0.3%
Zn (zinc)36.6–41%

CuZn40 Physical properties

Density8.18–8.35g/cm3

CuZn40 C28000 Hard Mechanical properties

Young’s modulus97–103GPa
Specific stiffness11.7–12.5MN.m/kg
Yield strength (elastic limit)150–160MPa
Tensile strength365–380MPa
Specific strength18.1–19.4kN.m/kg
Elongation28–30% strain
Compressive strength150–160MPa
Flexural modulus97–103GPa
Flexural strength (modulus of rupture)150–160MPa
Shear modulus35.9–38.1GPa
Bulk modulus105–111GPa
Poisson’s ratio0.34–0.35 
Shape factor29
Hardness – Vickers75–88HV
Elastic stored energy (springs)112–129kJ/m3
Fatigue strength at 10^7 cycles167–171MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
162–176MPa

CuZn40 Impact & fracture properties

Fracture toughness61.3–63.3MPa.m0.5
Toughness (G)37.2–40.5kJ/m2

CuZn40 C28000 Hard Thermal properties

Melting point882–902°C
Maximum service temperature180–190°C
Minimum service temperature-200  °C
Thermal conductivity122–129W/m.°C
Specific heat capacity376–378J/kg.°C
Thermal expansion coefficient19.4–20.6µstrain/°C
Thermal shock resistance73.5–81.7°C
Thermal distortion resistance6.02–6.54MW/m
Latent heat of fusion220–240kJ/kg

CuZn40 Electrical properties

Electrical resistivity6.61–7.24µohm.cm
Electrical conductivity23.8–26.1%IACS
Galvanic potential-0.34–-0.26V

CuZn40 Magnetic properties

Magnetic typeNon-magnetic

CuZn40 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3420–3530m/s
Mechanical loss coefficient (tan delta)1.56e-4–1.78e-4 

CuZn40 Processing properties

Metal castingUnsuitable
Metal cold formingLimited use
Metal hot formingExcellent
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed64 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor

CuZn40 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn40 C28000 Hard Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn40 Notes

CuZn40 C28000 Hard Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn40 Standards with similar compositions

Australia: 280 to AS 1567, C27400 to AS 2738, C28000 to AS 2738
Canada: HC.4.237(274) to CSA
Czech Republic: CuZn40 to CSN 423220
France: CuZn40 to NF A51-103, CuZn40 to NF A51-104
International: CuZn40 to ISO 1634, CuZn40 to ISO 1635, CuZn40 to ISO 1637, CuZn40 to ISO 1639, CuZn40 to ISO 426-1
Japan: C2800 BD to JIS H3250, C2800 BE to JIS H3250, C2800 T to JIS H3300, C2800 W to JIS H3260, C2801 P/R to JIS H3100, CuZn40 to JIS H3401
UK: CZ109 to BS 2872, CZ109 to BS 2874
USA: 60Cu-40Zn to QQ B-613, 60Cu-40Zn to QQ B-626, C27400, C27400 to ASTM B134, C27400 to ASTM B135M, C28000, C28000 to ASTM B111M, C28000 to ASTM B135M, C28000 to ASTM B36/B36M, UNS C27400, UNS C28000
Tradenames: BRASS, PIN WIRE, CERRO CF22, DELTA CF22 GENERAL PURPOSE ROD AND BAR, DELTA CF23 GENERAL PURPOSE ROD AND BAR, DELTA CF23 HIGH SPEED MACHINING ROD, FUCHS 2160, IMI 239, IMI 443, IMI 452 (MUNTZ METAL), IMI 453, MCKECHNIE SS SPECIAL, MUNTZ METAL, MUNTZ METAL NO. 3, PLUMRITE, PRYM 237, PRYM 265, REVERE ALLOY NO. 280C, SCOVILL ALLOY 280 MUNTZ METAL, SEAMLESS TUBING ALLOY, SVENSKA SM-1160, TITAN MUNTZ METAL, WIELAND-Z20, WIELAND-Z22