Home » Brass Alloys » CuZn39Pb2 (C37700) Leaded Forging Brass, Hot Worked Material Data Sheet
CuZn39Pb2 (C37700) Leaded Forging Brass, Hot Worked Material Data Sheet
CuZn39Pb2 (C37700) Leaded Forging Brass Material Data Sheet (Wrought, Hot Worked)
CuZn39Pb2 C37700 Hot Worked (Leaded Forging Brass) Overview
CuZn39Pb2 C37700 hot worked leaded forging brass is a wrought brass (UNS C37700), known as leaded forging brass. Condition: Hot worked. This CuZn39Pb2 C37700 hot worked leaded forging brass material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn39Pb2 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn39Pb2 brass parts in-house and inspects them before shipment.
CuZn39Pb2 C37700 Hot Worked (Leaded Forging Brass) Composition detail
Cu (copper)
56.7
–
62.3
%
Fe (iron)
0
–
0.3
%
Pb (lead)
1.5
–
2.5
%
Zn (zinc)
36.2
–
40.5
%
CuZn39Pb2 Physical properties
Density
8.18
–
8.35
g/cm3
CuZn39Pb2 C37700 Hot Worked (Leaded Forging Brass) Mechanical properties
Young’s modulus
97
–
103
GPa
Specific stiffness
11.7
–
12.5
MN.m/kg
Yield strength (elastic limit)
160
–
170
MPa
Tensile strength
380
–
400
MPa
Specific strength
19.3
–
20.6
kN.m/kg
Elongation
26
–
30
% strain
Compressive strength
160
–
170
MPa
Flexural modulus
97
–
103
GPa
Flexural strength (modulus of rupture)
160
–
170
MPa
Shear modulus
35.9
–
38.1
GPa
Bulk modulus
105
–
111
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
28
Hardness – Vickers
81
–
99
HV
Elastic stored energy (springs)
127
–
145
kJ/m3
Fatigue strength at 10^7 cycles
171
–
177
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
164
–
184
MPa
CuZn39Pb2 Impact & fracture properties
Fracture toughness
59.4
–
61.3
MPa.m0.5
Toughness (G)
34.9
–
38
kJ/m2
CuZn39Pb2 C37700 Hot Worked (Leaded Forging Brass) Thermal properties
Melting point
882
–
902
°C
Maximum service temperature
180
–
190
°C
Minimum service temperature
-170
–
-160
°C
Thermal conductivity
120
–
128
W/m.°C
Specific heat capacity
376
–
378
J/kg.°C
Thermal expansion coefficient
19.4
–
20.6
µstrain/°C
Thermal shock resistance
78.4
–
86.9
°C
Thermal distortion resistance
5.93
–
6.48
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn39Pb2 Electrical properties
Electrical resistivity
6.46
–
6.92
µohm.cm
Electrical conductivity
24.9
–
26.7
%IACS
Galvanic potential
-0.35
–
-0.27
V
CuZn39Pb2 Magnetic properties
Magnetic type
Non-magnetic
CuZn39Pb2 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3420
–
3530
m/s
Mechanical loss coefficient (tan delta)
1.38e-4
–
1.56e-4
CuZn39Pb2 Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Excellent
Metal press forming
Acceptable
Metal deep drawing
Limited use
Machining speed
91.4 m/min
Weldability Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor
CuZn39Pb2 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuZn39Pb2 C37700 Hot Worked (Leaded Forging Brass) Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible
CuZn39Pb2 Notes
CuZn39Pb2 C37700 Hot Worked (Leaded Forging Brass) Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn39Pb2 Standards with similar compositions
Denmark: 5167 to DS 3003
France: CuZn38Pb2 to NF A51-101, CuZn39Pb2 to NF A51-101
Germany: 2.038 to DIN, CuZn39Pb2 to DIN
International: CuZn38Pb2 to ISO 1634, CuZn38Pb2 to ISO 1635, CuZn38Pb2 to ISO 1637, CuZn38Pb2 to ISO 1638, CuZn38Pb2 to ISO 426-2
Japan: C3561 P/R to JIS H3100
Norway: 16135 to NS 16135
UK: CZ120 to BS 2870
USA: 60Cu-2.0Pb-37.5Zn to AMS 4614, 60Cu-38Zn-2Pb to MIL C-13351, 60Cu-38Zn-2Pb to QQ B-626, C37700, C37700 to ASTM B124M, C37700 to ASTM B283, C37700 to SAE J463, UNS C37700