CuZn39Pb2 (C37700) Leaded Clock Brass, Cold Worked Material Data Sheet

CuZn39Pb2 (C37700) Leaded Clock Brass Material Data Sheet (Wrought, Cold Worked)

CuZn39Pb2 C37700 Cold Worked Overview

CuZn39Pb2 C37700 cold worked is a wrought brass (UNS C37700), known as leaded clock brass. Condition: Cold worked. This CuZn39Pb2 C37700 cold worked material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn39Pb2 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn39Pb2 brass parts in-house and inspects them before shipment.

CuZn39Pb2 Designation

CuZn39Pb2, wrought
ConditionCold worked
UNS numberC37700
EN nameCW617N
ISO nameCuZn40Pb2

CuZn39Pb2 Typical uses

Hot forged components, high-speed machined, precision parts, taps, valves, fittings, door & window furniture, automobile components, clock & instrument gears, decorative items.

CuZn39Pb2 C37700 Cold Worked Composition detail

Cu (copper)56.7–62.3%
Fe (iron)0–0.3%
Pb (lead)1.5–2.5%
Zn (zinc)36.2–40.5%

CuZn39Pb2 Physical properties

Density8.18–8.35g/cm3

CuZn39Pb2 C37700 Cold Worked Mechanical properties

Young’s modulus97–103GPa
Specific stiffness11.7–12.5MN.m/kg
Yield strength (elastic limit)300–450MPa
Tensile strength450–560MPa
Specific strength36.3–54.4kN.m/kg
Elongation10–16% strain
Compressive strength300–450MPa
Flexural modulus97–103GPa
Flexural strength (modulus of rupture)300–450MPa
Shear modulus35.9–38.1GPa
Bulk modulus105–111GPa
Poisson’s ratio0.34–0.35 
Shape factor21
Hardness – Vickers85–110HV
Elastic stored energy (springs)466–980kJ/m3
Fatigue strength at 10^7 cycles191–220MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
165–255MPa

CuZn39Pb2 Impact & fracture properties

Fracture toughness31.7–42.2MPa.m0.5
Toughness (G)10.2–17.5kJ/m2

CuZn39Pb2 C37700 Cold Worked Thermal properties

Melting point882–902°C
Maximum service temperature180–190°C
Minimum service temperature-170–-160°C
Thermal conductivity120–128W/m.°C
Specific heat capacity376–378J/kg.°C
Thermal expansion coefficient19.4–20.6µstrain/°C
Thermal shock resistance150–226°C
Thermal distortion resistance5.93–6.48MW/m
Latent heat of fusion220–240kJ/kg

CuZn39Pb2 Electrical properties

Electrical resistivity6.17–6.61µohm.cm
Electrical conductivity26.1–27.9%IACS
Galvanic potential-0.35–-0.27V

CuZn39Pb2 Magnetic properties

Magnetic typeNon-magnetic

CuZn39Pb2 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3420–3530m/s
Mechanical loss coefficient (tan delta)2e-5–4.4e-5 

CuZn39Pb2 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed91.4 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor

CuZn39Pb2 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn39Pb2 C37700 Cold Worked Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn39Pb2 Notes

CuZn39Pb2 C37700 Cold Worked Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn39Pb2 Standards with similar compositions

Denmark: 5167 to DS 3003
France: CuZn38Pb2 to NF A51-101, CuZn39Pb2 to NF A51-101
Germany: 2.038 to DIN, CuZn39Pb2 to DIN
International: CuZn38Pb2 to ISO 1634, CuZn38Pb2 to ISO 1635, CuZn38Pb2 to ISO 1637, CuZn38Pb2 to ISO 1638, CuZn38Pb2 to ISO 426-2
Japan: C3561 P/R to JIS H3100
Norway: 16135 to NS 16135
UK: CZ120 to BS 2870
USA: 60Cu-2.0Pb-37.5Zn to AMS 4614, 60Cu-38Zn-2Pb to MIL C-13351, 60Cu-38Zn-2Pb to QQ B-626, C37700, C37700 to ASTM B124M, C37700 to ASTM B283, C37700 to SAE J463, UNS C37700
Tradenames: 3770, ACIMET C-3, BOHNALLOY R58NE, BOHNOLLOY R-58E, BRASS E-133, BRIDGEPORT NO. 134, DELTA S2 FORGING ROD, DELTA S2 GENERAL PURPOSE ROD AND BAR, DELTA S2 HIGH SPEED MACHINING ROD, ELBEBRONZE LBU, FORGING BRASS NO. 377, FORGING BRASS-377, IMI 455, IMI 458, KREIDLER MS 59/2, MCKECHNIE 226, MUELLER 3770, MUELLER 3771, MUELLER ALLOY C37700, REVERE ALLOY NO. 317, REVERE NO. 260, SCOVILL FORGING BRASS, ALLOY 377, SM-1459, TITAN NO. 36