CuZn36Pb3 (C36000) Free-Cutting Brass, Soft Material Data Sheet

CuZn36Pb3 (C36000) Free-Cutting Brass Material Data Sheet (Wrought, Soft)

CuZn36Pb3 C36000 Soft Overview

CuZn36Pb3 C36000 soft is a wrought brass (UNS C36000), known as free-cutting brass. Condition: Soft. This CuZn36Pb3 C36000 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn36Pb3 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn36Pb3 brass parts in-house and inspects them before shipment.

CuZn36Pb3 Designation

CuZn36Pb3, wrought
ConditionSoft
UNS numberC36000
EN nameCW603N
ISO nameCuZn36Pb3
JIS (Japanese) nameC3600

CuZn36Pb3 Typical uses

Machined parts on automatic lathes, bushes, bearings, screws, extrusions.

CuZn36Pb3 C36000 Soft Composition detail

Cu (copper)58.4–64.5%
Fe (iron)0–0.35%
Pb (lead)2.5–3.7%
Zn (zinc)33–37.5%

CuZn36Pb3 Physical properties

Density8.18–8.35g/cm3

CuZn36Pb3 C36000 Soft Mechanical properties

Young’s modulus98.9–105GPa
Specific stiffness11.9–12.7MN.m/kg
Yield strength (elastic limit)150–160MPa
Tensile strength360–400MPa
Specific strength18.1–19.4kN.m/kg
Elongation36–40% strain
Compressive strength150–160MPa
Flexural modulus98.9–105GPa
Flexural strength (modulus of rupture)150–160MPa
Shear modulus36.6–38.9GPa
Bulk modulus107–113GPa
Poisson’s ratio0.34–0.35 
Shape factor29
Hardness – Vickers75–80HV
Elastic stored energy (springs)110–126kJ/m3
Fatigue strength at 10^7 cycles165–177MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
153–191MPa

CuZn36Pb3 Impact & fracture properties

Fracture toughness61.3–63.3MPa.m0.5
Toughness (G)36.5–39.8kJ/m2

CuZn36Pb3 C36000 Soft Thermal properties

Melting point877–897°C
Maximum service temperature97–110°C
Minimum service temperature-273  °C
Thermal conductivity120–125W/m.°C
Specific heat capacity376–378J/kg.°C
Thermal expansion coefficient19.4–20.6µstrain/°C
Thermal shock resistance72.1–80.2°C
Thermal distortion resistance5.91–6.35MW/m
Latent heat of fusion220–240kJ/kg

CuZn36Pb3 Electrical properties

Electrical resistivity6.5–6.8µohm.cm
Electrical conductivity25.4–26.5%IACS
Galvanic potential-0.34–-0.26V

CuZn36Pb3 Magnetic properties

Magnetic typeNon-magnetic

CuZn36Pb3 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3460–3570m/s
Mechanical loss coefficient (tan delta)1.56e-4–1.78e-4 

CuZn36Pb3 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed104 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor

CuZn36Pb3 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Contains lead which lubricates, improving resistance.
Excellent
FlammabilityNon-flammable

CuZn36Pb3 C36000 Soft Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn36Pb3 Notes

CuZn36Pb3 C36000 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn36Pb3 Standards with similar compositions

Australia: 360 to AS 1567, C36000 to AS 2738
Canada: HC.5.ZP353(360) to CSA
Finland: CuZn36Pb3 to SFS 2922
France: CuZn36Pb3 to NF A51-105
International: CuZn36Pb3 to ISO 1637, CuZn36Pb3 to ISO 426-2
UK: CZ124 to BS 2874
USA: 61.5Cu-35.5Zn-3Pb to QQ B-613, 61.5Cu-35.5Zn-3Pb to QQ B-626, 61.5Cu-35Zn-3.1Pb to AMS 4610, C36000, C36000 to ASTM B16/B16M, C36000 to SAE J463, UNS C36000
Tradenames: 3600, ANACONDA 271, ANACONDA 360, ANSONIA ALLOY C36000, BOHNALLOY R61, BRIDGEPORT NO. 6, CERRO T5, DELTA T5 GENERAL PURPOSE ROD AND BAR, DELTA T5 HIGH SPEED MACHINING ROD, FREE CUTTING BRASS, COPPER ALLOY NO. 360, FREE CUTTING BRASS, SCOVILL 276, FREE CUTTING BRASS-360, FREE CUTTING YELLOW BRASS 271, IMI 441, LEDRITE 6, LEDRITE BRASS, MCKECHNIE YS, MUELLER 3600, NITTANY (FREE CUTTING) BRASS, NITTANY NO. 4, NITTANY NO. 49, NITTANY NO. 77, PRYM 261, RED TIP 360, REVERE FREE CUTTING BRASS, REVERE NO. 360, SCOVILL ALLOY 360, SCOVILL LEADED ROD 360, SVENSKA SM-1661, WIELAND-Z23