CuZn36 (C26800) Basis Brass, Soft Material Data Sheet

CuZn36 (C26800) Basis Brass Material Data Sheet (Wrought, Soft)

CuZn36 C26800 Soft Overview

CuZn36 C26800 soft is a wrought brass (UNS C26800), known as basis brass. Condition: Soft. This CuZn36 C26800 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn36 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn36 brass parts in-house and inspects them before shipment.

CuZn36 Designation

CuZn36, wrought
ConditionSoft
UNS numberC26800
EN nameCW506L
ISO nameCuZn33
JIS (Japanese) nameC2680

CuZn36 Typical uses

Good general cold-working alloy for spinnings & presswork but not deep-drawn items, cold-headed components, springs, car radiator tanks, hardware, fasteners, electrical items, wire brushes etc.

CuZn36 C26800 Soft Composition detail

Cu (copper)64–68.5%
Fe (iron)0–0.05%
Pb (lead)0–0.15%
Zn (zinc)31.3–36%

CuZn36 Physical properties

Density8.33–8.5g/cm3

CuZn36 C26800 Soft Mechanical properties

Young’s modulus97–103GPa
Specific stiffness11.5–12.3MN.m/kg
Yield strength (elastic limit)120–130MPa
Tensile strength325–340MPa
Specific strength14.2–15.5kN.m/kg
Elongation54–56% strain
Compressive strength120–130MPa
Flexural modulus97–103GPa
Flexural strength (modulus of rupture)120–130MPa
Shear modulus35.9–38.1GPa
Bulk modulus105–111GPa
Poisson’s ratio0.34–0.35 
Shape factor29
Hardness – Vickers64–75HV
Elastic stored energy (springs)71.8–84.8kJ/m3
Fatigue strength at 10^7 cycles155–159MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
150–165MPa

CuZn36 Impact & fracture properties

Fracture toughness67.9–70.4MPa.m0.5
Toughness (G)45.7–50.1kJ/m2

CuZn36 C26800 Soft Thermal properties

Melting point902–919°C
Maximum service temperature200–210°C
Minimum service temperature-273  °C
Thermal conductivity120–128W/m.°C
Specific heat capacity378–380J/kg.°C
Thermal expansion coefficient19–20.2µstrain/°C
Thermal shock resistance60.2–67.6°C
Thermal distortion resistance6.05–6.61MW/m
Latent heat of fusion220–240kJ/kg

CuZn36 Electrical properties

Electrical resistivity6.3–6.5µohm.cm
Electrical conductivity26.5–27.4%IACS
Galvanic potential-0.32–-0.24V

CuZn36 Magnetic properties

Magnetic typeNon-magnetic

CuZn36 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3390–3500m/s
Mechanical loss coefficient (tan delta)2.37e-4–2.78e-4 

CuZn36 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingExcellent
Metal press formingAcceptable
Metal deep drawingAcceptable
Machining speed57.9 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor

CuZn36 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn36 C26800 Soft Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn36 Notes

CuZn36 C26800 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn36 Standards with similar compositions

Australia: C26800 to AS 2738, C27000 to AS 2738
Canada: HC.4.Z34(268) to CSA HC.4.2
France: CuZn33 to NF A51-101, CuZn33 to NF A51-104
International: CuZn33 to ISO 1634, CuZn33 to ISO 1638, CuZn33 to ISO 426-1
Japan: C2680 P/R to JIS H3100, C2680 TW to JIS H3320, C2700 BD to JIS H3250, C2700 BE to JIS H3250, C2700 T to JIS H3300, C2700 W to JIS H3260
UK: CZ107 to BS 2870, CZ107 to BS 2873
USA: 65.5Cu-35.5Zn to AMS 4555, 65Cu-35Zn to QQ B-613, 65Cu-35Zn to QQ W-321, C26800, C26800 to ASTM B36/B36M, C26800 to ASTM B587, C26800 to SAE J463, C27000, C27000 to AMS 4712E, C27000 to ASTM B134, C27000 to ASTM B135M, C27000 to ASTM B587, C27000 to SAE J463, UNS C26800, UNS C27000
Tradenames: 2680, ANACONDA 268, ANACONDA 67, BRIDGEPORT NO. 1, COLD HEADING 4, DEGUSSA ALLOY, DIPPING BRASS, ENGLISH SPECULUM, EYELET BRASS, FEDERALOY RS-13, FUCHS 2167, HAMILTON METAL-B, IMI 233, JAPAN BRASS, LEADED TUBE BRASS 3301, MUELLER 2600, OLIN YELLOW BRASS 268, PRYM 227, REVERE ALLOY NO. 268, SCOVILL HIGH BRASS, 270, SEYMOUR 2265, SIN-CHU, SPRABRASS Y, TWO-TO-ONE, WESTERN ALLOY NO. 34, WIELAND-M33, YELLOW BRASS 59, YELLOW BRASS 66%