CuZn30 (C26000) Deep-Drawing/Cartridge Brass Material Data Sheet (Wrought, Soft)
CuZn30 C26000 Soft Overview
| CuZn30 C26000 soft is a wrought brass (UNS C26000), known as deep-drawing/cartridge brass. Condition: Soft. This CuZn30 C26000 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn30 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn30 brass parts in-house and inspects them before shipment. |
CuZn30 Designation
| CuZn30, wrought | |
| Condition | Soft |
| UNS number | C26000 |
| EN name | CW505L |
| ISO name | CuZn30 |
| GB (Chinese) name | H70 |
| JIS (Japanese) name | C2600 |
CuZn30 Typical uses
| Deep-drawn items including cartridge cases & heat exchangers (fresh clean water), cold-headed parts, hardware. |
CuZn30 C26000 Soft Composition detail
| Cu (copper) | 68.4 | – | 71.6 | % |
| Fe (iron) | 0 | – | 0.05 | % |
| Pb (lead) | 0 | – | 0.07 | % |
| Zn (zinc) | 28.4 | – | 31.5 | % |
CuZn30 Physical properties
| Density | 8.43 | – | 8.6 | g/cm3 |
CuZn30 C26000 Soft Mechanical properties
| Young’s modulus | 102 | – | 108 | GPa |
| Specific stiffness | 12 | – | 12.7 | MN.m/kg |
| Yield strength (elastic limit) | 110 | – | 120 | MPa |
| Tensile strength | 315 | – | 330 | MPa |
| Specific strength | 12.9 | – | 14.1 | kN.m/kg |
| Elongation | 50 | – | 52 | % strain |
| Compressive strength | 110 | – | 120 | MPa |
| Flexural modulus | 102 | – | 108 | GPa |
| Flexural strength (modulus of rupture) | 110 | – | 120 | MPa |
| Shear modulus | 37.7 | – | 40 | GPa |
| Bulk modulus | 110 | – | 117 | GPa |
| Poisson’s ratio | 0.34 | – | 0.35 | |
| Shape factor | 30 | |||
| Hardness – Vickers | 63 | – | 72 | HV |
| Elastic stored energy (springs) | 57.5 | – | 68.8 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 151 | – | 156 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 146 | – | 161 | MPa |
CuZn30 Impact & fracture properties
| Fracture toughness | 70.4 | – | 73.1 | MPa.m0.5 |
| Toughness (G) | 46.8 | – | 51.4 | kJ/m2 |
CuZn30 C26000 Soft Thermal properties
| Melting point | 952 | – | 967 | °C |
| Maximum service temperature | 200 | – | 210 | °C |
| Minimum service temperature | -273 | °C | ||
| Thermal conductivity | 118 | – | 124 | W/m.°C |
| Specific heat capacity | 379 | – | 381 | J/kg.°C |
| Thermal expansion coefficient | 18.4 | – | 19.6 | µstrain/°C |
| Thermal shock resistance | 54.3 | – | 61.2 | °C |
| Thermal distortion resistance | 6.12 | – | 6.63 | MW/m |
| Latent heat of fusion | 220 | – | 240 | kJ/kg |
CuZn30 Electrical properties
| Electrical resistivity | 6.17 | – | 6.61 | µohm.cm |
| Electrical conductivity | 26.1 | – | 27.9 | %IACS |
| Galvanic potential | -0.3 | – | -0.22 | V |
CuZn30 Magnetic properties
| Magnetic type | Non-magnetic |
CuZn30 Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 3460 | – | 3570 | m/s |
| Mechanical loss coefficient (tan delta) | 2.78e-4 | – | 3.31e-4 | |
CuZn30 Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Acceptable |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Excellent |
| Machining speed | 54.9 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
CuZn30 Durability
| Water (fresh) | Excellent |
| Water (salt) | Excellent |
| Weak acids | Acceptable |
| Strong acids | Unacceptable |
| Weak alkalis | Excellent |
| Strong alkalis | Excellent |
| Organic solvents | Excellent |
| Oxidation at 500C | Limited use |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) | Excellent |
| Flammability | Non-flammable |
CuZn30 C26000 Soft Corrosion resistance
| Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide | Highly susceptible |
CuZn30 Notes
| CuZn30 C26000 Soft Other notes |
| (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng. |
CuZn30 Standards with similar compositions
| Australia: 260 to AS 1566, 260 to AS 1567, C26000 to AS 2738 |
| Canada: HC.4.Z30(260) to CSA HC.4.2 |
| Czech Republic: CuZn30 to CSN 423210 |
| Finland: CuZn30 to SFS 2918 |
| France: CuZn30 to NF A51-101, CuZn30 to NF A51-103, CuZn30 to NF A51-104 |
| Germany: 2.0265 to DIN, CuZn30 to DIN |
| International: CuZn30 to ISO 1634, CuZn30 to ISO 1635, CuZn30 to ISO 1638, CuZn30 to ISO 426-1 |
| Japan: C2600 BD to JIS H3250, C2600 BE to JIS H3250, C2600 P/R to JIS H3100, C2600 T to JIS H3300, C2600 TW to JIS H3320, C2600 W to JIS H3260 |
| Mexico: LA-70 to DGN W-25 |
| Norway: 16115 to NS 16115 |
| Sweden: 5122-02 to SIS 145122, 5122-03 to SIS 145122, 5122-04 to SIS 145122, 5122-05 to SIS 145122 |
| UK: CZ106 to BS 2870, CZ106 to BS 2873, CZ106 to BS 2874, CZ106 to BS 2875 |
| USA: 70Cu-30Zn to AMS 4505, 70Cu-30Zn to MIL C-50, 70Cu-30Zn to MIL T-20219D, 70Cu-30Zn to MIL T-6945, 70Cu-30Zn to QQ B-613, 70Cu-30Zn to QQ B-626, C26000, C26000 to ASTM B129, C26000 to ASTM B134, C26000 to ASTM B135M, C26000 to ASTM B19, C26000 to ASTM B36/B36M, C26000 to ASTM B569, C26000 to ASTM B587, C26000 to ASTM B888, C26000 to SAE J463, UNS C26000 |
| Tradenames: 2600, 70/30 HIGH BRASS, ANACONDA 395, ANSONIA ALLOY C26000, BOLTOMET 518, BRASS, BRIDGEPORT 77, BRIDGEPORT NO. 37, BRIDGEPORT NO. 69, BRIDGEPORT NO. 77, CANZLER BRASS, CARTRIDGE BRASS, CARTRIDGE BRASS 260, CHASE HIGH STRENGTH TANK BRASS, COLONIAL NO. 407 (CDA 853), CUIVRE POLI, DELTA CF7 WIRE, F-37, FLEX-O-LOY, FUCHS 2170, GROMMET BRASS, HELMENT BRONZE, IMI 260, ISERLOHN, ISERLOHN BRASS, MCKECHNIE 311, OLIN CARTRIDGE BRASS, OUTOKUMPU MS70, PRYM 226, REVERE ALLOY NO. 260, REVERE CARTRIDGE BRASS, RIVERSIDE 61, RM 230 (CARTRIDGE BRASS), SCOVILL CARTRIDGE BRASS, 260, SEYMOUR 2270, SEYMOUR 270, TITAN NO. 75, TRIANGLE 70/30, VOLCO NO. 68, WESTERN NO. 30, WIELAND-M30, WOLVERINE CARTRIDGE BRASS 70%, YELLOW BRASS |