CuZn28 (C25600) Deep-Drawing/Cartridge Brass, Soft Material Data Sheet

CuZn28 (C25600) Deep-Drawing/Cartridge Brass Material Data Sheet (Wrought, Soft)

CuZn28 C25600 Soft Overview

CuZn28 C25600 soft is a wrought brass (UNS C25600), known as deep-drawing/cartridge brass. Condition: Soft. This CuZn28 C25600 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn28 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn28 brass parts in-house and inspects them before shipment.

CuZn28 Designation

CuZn28, wrought
ConditionSoft
UNS numberC25600
EN nameCW504L
ISO nameCuZn28
JIS (Japanese) nameC2560

CuZn28 Typical uses

Deep-drawn items including cartridge cases & heat exchangers (fresh clean water), cold-headed parts, hardware.

CuZn28 C25600 Soft Composition detail

Cu (copper)70.9–73.1%
Fe (iron)0–0.05%
Pb (lead)0–0.05%
Zn (zinc)26.9–29%

CuZn28 Physical properties

Density8.48–8.65g/cm3

CuZn28 C25600 Soft Mechanical properties

Young’s modulus109–115GPa
Specific stiffness12.7–13.5MN.m/kg
Yield strength (elastic limit)110–120MPa
Tensile strength315–330MPa
Specific strength12.8–14kN.m/kg
Elongation50–52% strain
Compressive strength110–120MPa
Flexural modulus109–115GPa
Flexural strength (modulus of rupture)110–120MPa
Shear modulus40.3–42.6GPa
Bulk modulus118–124GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers63–72HV
Elastic stored energy (springs)53.9–64.4kJ/m3
Fatigue strength at 10^7 cycles151–156MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
146–161MPa

CuZn28 Impact & fracture properties

Fracture toughness70.4–73.1MPa.m0.5
Toughness (G)43.9–48.1kJ/m2

CuZn28 C25600 Soft Thermal properties

Melting point957–972°C
Maximum service temperature200–210°C
Minimum service temperature-273  °C
Thermal conductivity120–126W/m.°C
Specific heat capacity380–382J/kg.°C
Thermal expansion coefficient17.9–19.1µstrain/°C
Thermal shock resistance52.3–58.9°C
Thermal distortion resistance6.39–6.92MW/m
Latent heat of fusion220–240kJ/kg

CuZn28 Electrical properties

Electrical resistivity5.89–6.46µohm.cm
Electrical conductivity26.7–29.3%IACS
Galvanic potential-0.3–-0.22V

CuZn28 Magnetic properties

Magnetic typeNon-magnetic

CuZn28 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3560–3670m/s
Mechanical loss coefficient (tan delta)2.78e-4–3.31e-4 

CuZn28 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingAcceptable
Metal press formingExcellent
Metal deep drawingExcellent
Machining speed51.8 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good

CuZn28 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn28 C25600 Soft Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn28 Notes

CuZn28 C25600 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn28 Standards with similar compositions

Europe: CW504L to CEN EN 12163
Germany: 2.0261 to DIN, CuZn28 to DIN
USA: C25600, UNS C25600
Tradenames: ANGSBURG, COMMON TOMBAC, FUCHS 2172, GOLD LEAF, LATTEN (LAITON)-2, LYON’S GOLD, MESSING 72, NEUSTADT, PRINCES METAL NO. 1, PRYM 225, REVERE NO. 158, RUSSIAN-3, SM-1072, SPRING WIRE BRASS, WIELAND-M28