Home » Brass Alloys » CuZn20Al2 (C68700) Aluminum Brass, Soft Material Data Sheet
CuZn20Al2 (C68700) Aluminum Brass, Soft Material Data Sheet
CuZn20Al2 (C68700) Aluminum Brass Material Data Sheet (Wrought, Soft)
CuZn20Al2 C68700 Soft Overview
CuZn20Al2 C68700 soft is a wrought brass (UNS C68700), known as aluminum brass. Condition: Soft. This CuZn20Al2 C68700 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn20Al2 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn20Al2 brass parts in-house and inspects them before shipment.
CuZn20Al2 Designation
CuZn20Al2, wrought
Condition
Soft
UNS number
C68700
ISO name
CuZn20Al2
CuZn20Al2 Typical uses
Heat exchangers, oil-tanker heating coils, marine equipment requiring good resistance to corrosion & erosion.
CuZn20Al2 C68700 Soft Composition detail
Al (aluminum)
1.8
–
2.5
%
As (arsenic)
0.02
–
0.06
%
Cu (copper)
75.1
–
79.9
%
Fe (iron)
0
–
0.06
%
Pb (lead)
0
–
0.07
%
Zn (zinc)
18.3
–
22.2
%
CuZn20Al2 Physical properties
Density
8.38
–
8.55
g/cm3
CuZn20Al2 C68700 Soft Mechanical properties
Young’s modulus
107
–
113
GPa
Specific stiffness
12.6
–
13.4
MN.m/kg
Yield strength (elastic limit)
115
–
125
MPa
Tensile strength
315
–
340
MPa
Specific strength
13.6
–
14.8
kN.m/kg
Elongation
58
–
60
% strain
Compressive strength
115
–
125
MPa
Flexural modulus
107
–
113
GPa
Flexural strength (modulus of rupture)
115
–
125
MPa
Shear modulus
39.6
–
41.8
GPa
Bulk modulus
116
–
122
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
30
Hardness – Vickers
72
–
78
HV
Elastic stored energy (springs)
60
–
71.2
kJ/m3
Fatigue strength at 10^7 cycles
151
–
159
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
143
–
168
MPa
CuZn20Al2 Impact & fracture properties
Fracture toughness
69.1
–
71.7
MPa.m0.5
Toughness (G)
43.1
–
47.1
kJ/m2
CuZn20Al2 C68700 Soft Thermal properties
Melting point
977
–
992
°C
Maximum service temperature
180
–
190
°C
Minimum service temperature
-200
°C
Thermal conductivity
96.4
–
104
W/m.°C
Specific heat capacity
378
–
380
J/kg.°C
Thermal expansion coefficient
17.9
–
19.1
µstrain/°C
Thermal shock resistance
55.6
–
62.5
°C
Thermal distortion resistance
5.16
–
5.71
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn20Al2 Electrical properties
Electrical resistivity
7.24
–
7.76
µohm.cm
Electrical conductivity
22.2
–
23.8
%IACS
Galvanic potential
-0.28
–
-0.2
V
CuZn20Al2 Magnetic properties
Magnetic type
Non-magnetic
CuZn20Al2 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3550
–
3660
m/s
Mechanical loss coefficient (tan delta)
2.56e-4
–
3.02e-4
CuZn20Al2 Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Limited use
Metal press forming
Acceptable
Metal deep drawing
Acceptable
Machining speed
61 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
CuZn20Al2 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuZn20Al2 C68700 Soft Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible
CuZn20Al2 Notes
CuZn20Al2 C68700 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn20Al2 Standards with similar compositions
Australia: 687 to AS 1572, C68700 to AS 2738
Denmark: 5217 to DS 3003
Europe: CW702R to CEN EN 12449, CW702R to CEN EN 12451, CW702R to CEN EN 12452, CW702R to CEN EN 1652, CW702R to CEN EN 1653
Finland: CuZn20A12 to SFS 2928
International: CuZn20Al2 to ISO 1634, CuZn20Al2 to ISO 1635, CuZn20Al2 to ISO 426-1
Japan: C6870 T to JIS H3300, C6871 T to JIS H3300
South Africa: Cu-Zn21Al2 to SABS 460
Sweden: 5217-02 to SIS 145217, 5217-12 to SIS 145217
UK: CZ110 to BS 2870, CZ110 to BS 2871, CZ110 to BS 2875
USA: C68700, C68700 to ASTM B111M, C68700 to ASTM B359M, C68700 to ASTM B395M, C68700 to ASTM B543M, UNS C68700
Tradenames: ALUMINUM BRASS, BRIDGEPORT 54, BRIDGEPORT NO. 54, CUZINAL, DELTABRA, HECORROS 76, NORANDA 6870, SCOVILL ALLOY 774 ALUMINUM BRASS TYPE B, SCOVILL ALLOY 787 ALUMINUM BRASS TYPE B, SCOVILL ALUMINUM BRASS TYPE A, YORCALBRO (ALUMINUM BRASS)