CuZn10 (C22000) Gilding Metal Material Data Sheet (Wrought, Soft)
CuZn10 C22000 Soft Overview
| CuZn10 C22000 soft is a wrought brass (UNS C22000), known as gilding metal. Condition: Soft. This CuZn10 C22000 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn10 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn10 brass parts in-house and inspects them before shipment. |
CuZn10 Designation
| CuZn10, wrought | |
| Condition | Soft |
| UNS number | C22000 |
| EN name | CW501L |
| ISO name | CuZn10 |
| GB (Chinese) name | H90 |
| JIS (Japanese) name | C2200 |
CuZn10 Typical uses
| Architectural & decorative items, jewelry, enameled & brazed parts. |
CuZn10 C22000 Soft Composition detail
| Cu (copper) | 88.9 | – | 91.1 | % |
| Fe (iron) | 0 | – | 0.05 | % |
| Pb (lead) | 0 | – | 0.05 | % |
| Zn (zinc) | 8.9 | – | 11 | % |
CuZn10 Physical properties
| Density | 8.63 | – | 8.8 | g/cm3 |
CuZn10 C22000 Soft Mechanical properties
| Young’s modulus | 116 | – | 124 | GPa |
| Specific stiffness | 13.3 | – | 14.3 | MN.m/kg |
| Yield strength (elastic limit) | 90 | – | 100 | MPa |
| Tensile strength | 270 | – | 280 | MPa |
| Specific strength | 10.3 | – | 11.5 | kN.m/kg |
| Elongation | 46 | – | 48 | % strain |
| Compressive strength | 90 | – | 100 | MPa |
| Flexural modulus | 116 | – | 124 | GPa |
| Flexural strength (modulus of rupture) | 90 | – | 100 | MPa |
| Shear modulus | 42.9 | – | 45.9 | GPa |
| Bulk modulus | 125 | – | 134 | GPa |
| Poisson’s ratio | 0.34 | – | 0.35 | |
| Shape factor | 30 | |||
| Hardness – Vickers | 63 | – | 68 | HV |
| Elastic stored energy (springs) | 33.7 | – | 41.8 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 137 | – | 140 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 133 | – | 144 | MPa |
CuZn10 Impact & fracture properties
| Fracture toughness | 76 | – | 79.2 | MPa.m0.5 |
| Toughness (G) | 47.6 | – | 52.9 | kJ/m2 |
CuZn10 C22000 Soft Thermal properties
| Melting point | 1030 | – | 1040 | °C |
| Maximum service temperature | 200 | – | 210 | °C |
| Minimum service temperature | -273 | °C | ||
| Thermal conductivity | 185 | – | 192 | W/m.°C |
| Specific heat capacity | 381 | – | 383 | J/kg.°C |
| Thermal expansion coefficient | 16.5 | – | 17.5 | µstrain/°C |
| Thermal shock resistance | 43.5 | – | 49.8 | °C |
| Thermal distortion resistance | 10.7 | – | 11.5 | MW/m |
| Latent heat of fusion | 220 | – | 240 | kJ/kg |
CuZn10 Electrical properties
| Electrical resistivity | 3.8 | – | 3.98 | µohm.cm |
| Electrical conductivity | 43.3 | – | 45.4 | %IACS |
| Galvanic potential | -0.23 | – | -0.15 | V |
CuZn10 Magnetic properties
| Magnetic type | Non-magnetic |
CuZn10 Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 3650 | – | 3780 | m/s |
| Mechanical loss coefficient (tan delta) | 4e-4 | – | 4.94e-4 | |
CuZn10 Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Acceptable |
| Metal hot forming | Limited use |
| Metal press forming | Acceptable |
| Metal deep drawing | Acceptable |
| Machining speed | 42.7 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
CuZn10 Durability
| Water (fresh) | Excellent |
| Water (salt) | Excellent |
| Weak acids | Acceptable |
| Strong acids | Unacceptable |
| Weak alkalis | Excellent |
| Strong alkalis | Excellent |
| Organic solvents | Excellent |
| Oxidation at 500C | Limited use |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) | Excellent |
| Flammability | Non-flammable |
CuZn10 C22000 Soft Corrosion resistance
| Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide | Susceptible |
CuZn10 Notes
| CuZn10 C22000 Soft Other notes |
| (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng. |
CuZn10 Standards with similar compositions
| Australia: 220 to AS 1566, 220 to AS 1567, 220A to AS 1566, C22000 to AS 2738 |
| Canada: HC.4.Z10(220) to CSA HC.4.2 |
| Czech Republic: CuZn10 to CSN 423201 |
| Finland: CuZn10 to SFS 2915 |
| France: CuZn10 to NF A51-101, CuZn10 to NF A51-103, CuZn10 to NF A51-104 |
| Germany: 2.023 to DIN, CuZn10 to DIN |
| International: CuZn10 to ISO 1634, CuZn10 to ISO 1638, CuZn10 to ISO 426-1 |
| Japan: C2200 P/R to JIS H3100, C2200 T to JIS H3300, C2200 W to JIS H3260 |
| Norway: 16106 to NS 16106 |
| UK: CZ101 to BS 2870, CZ101 to BS 2873 |
| USA: 90Cu-10Zn to MIL B-20292, 90Cu-10Zn to MIL C-21768, 90Cu-10Zn to MIL C-3383, 90Cu-10Zn to MIL T-52069, C22000, C22000 to ASTM B130, C22000 to ASTM B131, C22000 to ASTM B134, C22000 to ASTM B135M, C22000 to ASTM B36/B36M, C22000 to ASTM B372, C22000 to ASTM B587, C22000 to ASTM B694, C22000 to SAE J463, UNS C22000 |
| Tradenames: 2200, 90/10 COMMERCIAL BRONZE, ANACONDA 220, ANSONIA ALLOY C22000, BEST BRONZE, BOLTOMET 510, BRIDGEPORT NO. 25, BURR-B, CAP GILDING, COLONIAL NO. 407.5 (CDA 834), COMMERCIAL BRONZE, COMMERCIAL BRONZE 25, FUCHS 2190, MCKECHNIE E78, MESSING 90, OLIN COMMERCIAL BRONZE, OUTOKUMPU MS90, PRYM 222, REVERE COMMERCIAL BRONZE, RICH GOLD METAL, RIVERSIDE 63, RM 210, SCOVILL COMMERCIAL BRONZE, ALLOY 220, SEYMOUR 2290, SEYMOUR 290, SINTALOY Z-901, VOLCO NO. 30, WESTERN ALLOY NO. 10, WIELAND-M10, WOLVERINE COMMERCIAL BRONZE 90% |