CuZn40Pb2 (C38000) Brass, Pressure Die Cast Material Data Sheet

CuZn40Pb2 (C38000) Brass Material Data Sheet (Cast, Pressure Die Cast)

CuZn40Pb2 C38000 Pressure Die Cast Overview

CuZn40Pb2 C38000 pressure die cast is a cast brass (UNS C38000). Condition: Pressure Die Cast. This CuZn40Pb2 C38000 pressure die cast material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn40Pb2 brass castings from Turkey (Türkiye)? Modulus Metal supplies CuZn40Pb2 brass castings with in-house CNC machining and inspects them before shipment.

CuZn40Pb2 Designation

CuZn40Pb2
UNS numberC38000

CuZn40Pb2 Typical uses

Accurate general-purpose pressure-cast items, free-cutting.

CuZn40Pb2 C38000 Pressure Die Cast Composition detail

Al (aluminum)0–0.5%
Cu (copper)52.8–62.1%
Fe (iron)0–0.35%
Pb (lead)1.5–2.5%
Sn (tin)0–0.3%
Zn (zinc)36.4–43.5%

CuZn40Pb2 Physical properties

Density7.92–8.08g/cm3

CuZn40Pb2 C38000 Pressure Die Cast Mechanical properties

Young’s modulus91.1–92.9GPa
Specific stiffness11.3–11.7MN.m/kg
Yield strength (elastic limit)90–120MPa
Tensile strength280–370MPa
Specific strength11.2–15kN.m/kg
Elongation25–40% strain
Compressive strength90–120MPa
Flexural modulus91.1–92.9GPa
Flexural strength (modulus of rupture)90–120MPa
Shear modulus33.7–34.4GPa
Bulk modulus98.4–100GPa
Poisson’s ratio0.34–0.35 
Shape factor29
Hardness – Vickers60–70HV
Elastic stored energy (springs)44.8–76.9kJ/m3
Fatigue strength at 10^7 cycles140–168MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
116–203MPa

CuZn40Pb2 Impact & fracture properties

Fracture toughness70.4–79.2MPa.m0.5
Toughness (G)54–68kJ/m2

CuZn40Pb2 C38000 Pressure Die Cast Thermal properties

Melting point882–902°C
Maximum service temperature120–130°C
Minimum service temperature-273  °C
Thermal conductivity122–129W/m.°C
Specific heat capacity373–375J/kg.°C
Thermal expansion coefficient20.1–20.5µstrain/°C
Thermal shock resistance48.2–64.3°C
Thermal distortion resistance6–6.37MW/m
Latent heat of fusion220–240kJ/kg

CuZn40Pb2 Electrical properties

Electrical resistivity9.12–10µohm.cm
Electrical conductivity17.2–18.9%IACS
Galvanic potential-0.36–-0.28V

CuZn40Pb2 Magnetic properties

Magnetic typeNon-magnetic

CuZn40Pb2 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3370–3420m/s
Mechanical loss coefficient (tan delta)2.78e-4–4.94e-4 

CuZn40Pb2 Processing properties

Metal castingAcceptable
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed94.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor

CuZn40Pb2 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn40Pb2 C38000 Pressure Die Cast Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn40Pb2 Notes

CuZn40Pb2 C38000 Pressure Die Cast Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn40Pb2 Standards with similar compositions

Europe: CB755S to CEN EN 1982, CC755S to CEN EN 1982
Tradenames: MCGILL BRASS PRESSURE CASTING ALLOY