CuZn15As0.2 (C23000) Brazable Brass, Sand-Cast Material Data Sheet

CuZn15As0.2 (C23000) Brazable Brass Material Data Sheet (Cast, Sand-Cast)

CuZn15As0.2 C23000 Sand-Cast Overview

CuZn15As0.2 C23000 sand-cast is a cast brass (UNS C23000), known as brazable brass. Condition: Sand-Cast. This CuZn15As0.2 C23000 sand-cast material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn15As0.2 brass castings from Turkey (Türkiye)? Modulus Metal supplies CuZn15As0.2 brass castings with in-house CNC machining and inspects them before shipment.

CuZn15As0.2 Designation

CuZn15As0.2
UNS numberC23000
EN nameCW502L
ISO nameCuZn15
GB (Chinese) nameH85
JIS (Japanese) nameC2300

CuZn15As0.2 Typical uses

Marine fittings etc. to be brazed, flanges & end-plates, costume jewelry.

CuZn15As0.2 C23000 Sand-Cast Composition detail

Al (aluminum)0–0.01%
As (arsenic)0.05–0.2%
Cu (copper)83–88%
Fe (iron)0–0.15%
Mn (manganese)0–0.1%
Ni (nickel)0–0.1%
Pb (lead)0–0.5%
Si (silicon)0–0.02%
Sn (tin)0–0.3%
Zn (zinc)11.3–17%

CuZn15As0.2 Physical properties

Density8.51–8.69g/cm3

CuZn15As0.2 C23000 Sand-Cast Mechanical properties

Young’s modulus99–101GPa
Specific stiffness11.5–11.8MN.m/kg
Yield strength (elastic limit)80–110MPa
Tensile strength170–190MPa
Specific strength9.3–12.8kN.m/kg
Elongation18–40% strain
Compressive strength80–110MPa
Flexural modulus99–101GPa
Flexural strength (modulus of rupture)80–110MPa
Shear modulus36.6–37.4GPa
Bulk modulus107–109GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers45–60HV
Elastic stored energy (springs)32.7–59.2kJ/m3
Fatigue strength at 10^7 cycles101–109MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
89.3–123MPa

CuZn15As0.2 Impact & fracture properties

Fracture toughness73.1–82.6MPa.m0.5
Toughness (G)53.6–68kJ/m2

CuZn15As0.2 C23000 Sand-Cast Thermal properties

Melting point1010–1020°C
Maximum service temperature120–130°C
Minimum service temperature-273  °C
Thermal conductivity156–161W/m.°C
Specific heat capacity380–382J/kg.°C
Thermal expansion coefficient17.8–18.2µstrain/°C
Thermal shock resistance44.4–61.1°C
Thermal distortion resistance8.64–8.97MW/m
Latent heat of fusion220–240kJ/kg

CuZn15As0.2 Electrical properties

Electrical resistivity5.89–6.92µohm.cm
Electrical conductivity24.9–29.3%IACS
Galvanic potential-0.25–-0.17V

CuZn15As0.2 Magnetic properties

Magnetic typeNon-magnetic

CuZn15As0.2 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3390–3430m/s
Mechanical loss coefficient (tan delta)3.31e-4–6.25e-4 

CuZn15As0.2 Processing properties

Metal castingAcceptable
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed76.2 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Good

CuZn15As0.2 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn15As0.2 C23000 Sand-Cast Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Susceptible

CuZn15As0.2 Notes

CuZn15As0.2 C23000 Sand-Cast Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn15As0.2 Standards with similar compositions

Australia: 837D to AS 1565, C83700 to AS 2738
Europe: CB760S to CEN EN 1982, CC760S to CEN EN 1982
Germany: 2.0241 to DIN, G-CuZn15 to DIN
South Africa: Cu-Zn14 to SABS 200
USA: UNS C83700