Home » Brass Alloys » CuZn5 (C21000) Gilding Metal, Soft Material Data Sheet
CuZn5 (C21000) Gilding Metal, Soft Material Data Sheet
CuZn5 (C21000) Gilding Metal Material Data Sheet (Wrought, Soft)
CuZn5 C21000 Soft Overview
CuZn5 C21000 soft is a wrought brass (UNS C21000), known as gilding metal. Condition: Soft. This CuZn5 C21000 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn5 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn5 brass parts in-house and inspects them before shipment.
CuZn5 Designation
CuZn5, wrought
Condition
Soft
UNS number
C21000
EN name
CW500L
ISO name
CuZn5
GB (Chinese) name
H96
JIS (Japanese) name
C2100
CuZn5 Typical uses
Ammunition caps.
CuZn5 C21000 Soft Composition detail
Cu (copper)
93.9
–
96.1
%
Fe (iron)
0
–
0.05
%
Pb (lead)
0
–
0.03
%
Zn (zinc)
3.92
–
6
%
CuZn5 Physical properties
Density
8.59
–
8.76
g/cm3
CuZn5 C21000 Soft Mechanical properties
Young’s modulus
116
–
124
GPa
Specific stiffness
13.4
–
14.3
MN.m/kg
Yield strength (elastic limit)
90
–
100
MPa
Tensile strength
260
–
270
MPa
Specific strength
10.4
–
11.5
kN.m/kg
Elongation
43
–
45
% strain
Compressive strength
90
–
100
MPa
Flexural modulus
116
–
124
GPa
Flexural strength (modulus of rupture)
90
–
100
MPa
Shear modulus
42.9
–
45.9
GPa
Bulk modulus
125
–
134
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
30
Hardness – Vickers
58
–
62
HV
Elastic stored energy (springs)
33.7
–
41.8
kJ/m3
Fatigue strength at 10^7 cycles
134
–
137
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
130
–
141
MPa
CuZn5 Impact & fracture properties
Fracture toughness
76
–
79.2
MPa.m0.5
Toughness (G)
47.6
–
52.9
kJ/m2
CuZn5 C21000 Soft Thermal properties
Melting point
1060
–
1070
°C
Maximum service temperature
200
–
210
°C
Minimum service temperature
-200
°C
Thermal conductivity
230
–
235
W/m.°C
Specific heat capacity
381
–
383
J/kg.°C
Thermal expansion coefficient
16.5
–
17.5
µstrain/°C
Thermal shock resistance
43.5
–
49.8
°C
Thermal distortion resistance
13.3
–
14.1
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn5 Electrical properties
Electrical resistivity
3.02
–
3.16
µohm.cm
Electrical conductivity
54.6
–
57.1
%IACS
Galvanic potential
-0.22
–
-0.14
V
CuZn5 Magnetic properties
Magnetic type
Non-magnetic
CuZn5 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3650
–
3780
m/s
Mechanical loss coefficient (tan delta)
4e-4
–
4.94e-4
CuZn5 Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Acceptable
Metal press forming
Excellent
Metal deep drawing
Acceptable
Machining speed
39.6 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
CuZn5 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuZn5 C21000 Soft Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Susceptible
CuZn5 Notes
CuZn5 C21000 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn5 Standards with similar compositions
Australia: C21000 to AS 2738
Canada: HC.4.Z5(210) to CSA HC.4.2
Europe: CW500L to CEN EN 12163, CW500L to CEN EN 12449, CW500L to CEN EN 1652
France: CuZn5 to NF A51-101
Germany: 2.022 to DIN, CuZn5 to DIN
International: CuZn5 to ISO 1634, CuZn5 to ISO 1638, CuZn5 to ISO 426-1
Japan: C2100 P/R to JIS H3100, C2100 W to JIS H3260
USA: 95Cu-5Zn to MIL C-21768, 95Cu-5Zn to QQ W-321, C21000, C21000 to ASTM B134, C21000 to ASTM B36/B36M, C21000 to ASTM B587, C21000 to CDA Datasheet, C21000 to SAE J463, UNS C21000