Home » Brass Alloys » CuZn38Sn1 (C46400) Naval Brass, Hard Material Data Sheet
CuZn38Sn1 (C46400) Naval Brass, Hard Material Data Sheet
CuZn38Sn1 (C46400) Naval Brass Material Data Sheet (Wrought, Hard)
CuZn38Sn1 C46400 Hard Overview
CuZn38Sn1 C46400 hard is a wrought brass (UNS C46400), known as naval brass. Condition: Hard. This CuZn38Sn1 C46400 hard material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn38Sn1 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn38Sn1 brass parts in-house and inspects them before shipment.
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
171
–
181
MPa
CuZn38Sn1 Impact & fracture properties
Fracture toughness
59.4
–
61.3
MPa.m0.5
Toughness (G)
34.2
–
37.3
kJ/m2
CuZn38Sn1 C46400 Hard Thermal properties
Melting point
902
–
919
°C
Maximum service temperature
150
–
160
°C
Minimum service temperature
-200
°C
Thermal conductivity
120
–
128
W/m.°C
Specific heat capacity
376
–
378
J/kg.°C
Thermal expansion coefficient
19.4
–
20.6
µstrain/°C
Thermal shock resistance
76.9
–
85.2
°C
Thermal distortion resistance
5.93
–
6.48
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn38Sn1 Electrical properties
Electrical resistivity
6.46
–
6.92
µohm.cm
Electrical conductivity
24.9
–
26.7
%IACS
Galvanic potential
-0.34
–
-0.26
V
CuZn38Sn1 Magnetic properties
Magnetic type
Non-magnetic
CuZn38Sn1 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3450
–
3570
m/s
Mechanical loss coefficient (tan delta)
1.38e-4
–
1.56e-4
CuZn38Sn1 Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Acceptable
Metal press forming
Acceptable
Metal deep drawing
Limited use
Machining speed
61 m/min
Weldability Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Good
CuZn38Sn1 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuZn38Sn1 C46400 Hard Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible
CuZn38Sn1 Notes
CuZn38Sn1 C46400 Hard Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn38Sn1 Standards with similar compositions
Australia: C46400 to AS 2738
Canada: HC.4.ZT381P to CSA HC.4.9, HC.4.ZT391(464) to CSA HC.4.9
Europe: CW719R to CEN EN 12163, CW719R to CEN EN 12165, CW719R to CEN EN 12167, CW719R to CEN EN 12420, CW719R to CEN EN 1653
Japan: C4640 P to JIS H3100, C4641 BD to JIS H3250, C4641 BE to JIS H3250
USA: 464 to QQ B-639B, 60.5Cu-38.7Zn-0.8Sn to AMS 4611, 60.5Cu-38Zn-.8Sn.7Pb to QQ B-626, 60.5Cu-38Zn-.8Sn.7Pb to QQ B-637, 60Cu-37.5Zn1.8Pb.7Sn to QQ B-626, 60Cu-37.5Zn1.8Pb.7Sn to QQ B-637, 60Cu-39.2Zn-.8Sn to ASME SB171, 60Cu-39.2Zn-.8Sn to QQ B-637, C46400, C46400 to ASTM B124M, C46400 to ASTM B171/B171M, C46400 to ASTM B21M, C46400 to ASTM B283, C46400 to SAE J463, UNS C46400