CuZn36Pb2 (C35300) Leaded Clock Brass, Soft Material Data Sheet

CuZn36Pb2 (C35300) Leaded Clock Brass Material Data Sheet (Wrought, Soft)

CuZn36Pb2 C35300 Soft Overview

CuZn36Pb2 C35300 soft is a wrought brass (UNS C35300), known as leaded clock brass. Condition: Soft. This CuZn36Pb2 C35300 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn36Pb2 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn36Pb2 brass parts in-house and inspects them before shipment.

CuZn36Pb2 Designation

CuZn36Pb2, wrought
ConditionSoft
UNS numberC35300
EN nameCW606N
ISO nameCuZn37Pb2
JIS (Japanese) nameC3530

CuZn36Pb2 Typical uses

Machined & blanked parts, spark plugs & battery terminals, dials & engraved plates.

CuZn36Pb2 C35300 Soft Composition detail

Cu (copper)58.9–64.1%
Fe (iron)0–0.1%
Pb (lead)1.5–2.5%
Zn (zinc)34.4–38.5%

CuZn36Pb2 Physical properties

Density8.23–8.4g/cm3

CuZn36Pb2 C35300 Soft Mechanical properties

Young’s modulus98.9–105GPa
Specific stiffness11.9–12.6MN.m/kg
Yield strength (elastic limit)120–130MPa
Tensile strength325–340MPa
Specific strength14.4–15.7kN.m/kg
Elongation40–45% strain
Compressive strength120–130MPa
Flexural modulus98.9–105GPa
Flexural strength (modulus of rupture)120–130MPa
Shear modulus36.6–38.9GPa
Bulk modulus107–113GPa
Poisson’s ratio0.34–0.35 
Shape factor29
Hardness – Vickers59–72HV
Elastic stored energy (springs)70.4–83.2kJ/m3
Fatigue strength at 10^7 cycles155–159MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
149–165MPa

CuZn36Pb2 Impact & fracture properties

Fracture toughness67.9–70.4MPa.m0.5
Toughness (G)44.8–49.1kJ/m2

CuZn36Pb2 C35300 Soft Thermal properties

Melting point905–922°C
Maximum service temperature180–190°C
Minimum service temperature-170–-160°C
Thermal conductivity121–129W/m.°C
Specific heat capacity377–379J/kg.°C
Thermal expansion coefficient19.1–20.3µstrain/°C
Thermal shock resistance58.7–66°C
Thermal distortion resistance6.07–6.63MW/m
Latent heat of fusion220–240kJ/kg

CuZn36Pb2 Electrical properties

Electrical resistivity6.46–6.92µohm.cm
Electrical conductivity24.9–26.7%IACS
Galvanic potential-0.34–-0.26V

CuZn36Pb2 Magnetic properties

Magnetic typeNon-magnetic

CuZn36Pb2 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3450–3560m/s
Mechanical loss coefficient (tan delta)2.37e-4–2.78e-4 

CuZn36Pb2 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed88.4 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor

CuZn36Pb2 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn36Pb2 C35300 Soft Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn36Pb2 Notes

CuZn36Pb2 C35300 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn36Pb2 Standards with similar compositions

Australia: 353 to AS 1567, C35300 to AS 2738
Canada: HC.4.ZP352 to CSA HC.4.3
France: CuZn35Pb2 to NF A51-105
International: CuZn35Pb2 to ISO 1634, CuZn35Pb2 to ISO 1637, CuZn35Pb2 to ISO 1638, CuZn35Pb2 to ISO 426-2
UK: CZ119 to BS 2870, CZ119 to BS 2871, CZ119 to BS 2873, CZ119 to BS 2874
USA: C35300, C35300 to ASTM B121/B121M, C35300 to ASTM B453M, C35300 to CDA Datasheet, UNS C35300
Tradenames: 3530, ANSONIA ALLOY C35300, BOHNALLOY R63, BOOTH B76, BOSCH (ME-16), BRIDGEPORT NO. 62, CLOCK BRASS-243, DELTA TR1 GENERAL PURPOSE ROD AND BAR, DELTA TR1 HIGH SPEED MACHINING ROD, HIGH LEADED BRASS 353, HIGH LEADED BRASS 3531, HIGH LEADED BRASS 62, HIGH LEADED BRASS 62%, HOOKER BRASS, IMI 433, LEADED FLANGING BRASS, LEDRITE 2, MCKECHNIE 20, MESSING 63PB, MUELLER 3450, NITTANY NO. 2, NITTANY NO. 38, OLIN HIGH LEADED BRASS 353, PRYM 263, RM 433, WESTERN ALLOY NO. 68, WESTERN HIGH LEADED BRASS #68, WIELAND-Z14, WIELAND-Z21