CuZn34Pb1 (C34000) Leaded Clock Brass, Soft Material Data Sheet

CuZn34Pb1 (C34000) Leaded Clock Brass Material Data Sheet (Wrought, Soft)

CuZn34Pb1 C34000 Soft Overview

CuZn34Pb1 C34000 soft is a wrought brass (UNS C34000), known as leaded clock brass. Condition: Soft. This CuZn34Pb1 C34000 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn34Pb1 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn34Pb1 brass parts in-house and inspects them before shipment.

CuZn34Pb1 Designation

CuZn34Pb1, wrought
ConditionSoft
UNS numberC34000
EN nameCW600N
ISO nameCuZn35Pb1
JIS (Japanese) nameC3501

CuZn34Pb1 Typical uses

Headed or blanked parts, instrument & clock items, keys, printers’ matrices.

CuZn34Pb1 C34000 Soft Composition detail

Cu (copper)62–65%
Fe (iron)0–0.1%
Pb (lead)0.8–1.5%
Zn (zinc)33.4–37.2%

CuZn34Pb1 Physical properties

Density8.23–8.4g/cm3

CuZn34Pb1 C34000 Soft Mechanical properties

Young’s modulus101–107GPa
Specific stiffness12.1–12.9MN.m/kg
Yield strength (elastic limit)110–120MPa
Tensile strength315–330MPa
Specific strength13.2–14.4kN.m/kg
Elongation40–45% strain
Compressive strength110–120MPa
Flexural modulus101–107GPa
Flexural strength (modulus of rupture)110–120MPa
Shear modulus37.4–39.6GPa
Bulk modulus109–116GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers59–72HV
Elastic stored energy (springs)58.1–69.4kJ/m3
Fatigue strength at 10^7 cycles151–156MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
145–162MPa

CuZn34Pb1 Impact & fracture properties

Fracture toughness70.4–73.1MPa.m0.5
Toughness (G)47.2–51.9kJ/m2

CuZn34Pb1 C34000 Soft Thermal properties

Melting point927–942°C
Maximum service temperature180–190°C
Minimum service temperature-170–-160°C
Thermal conductivity118–124W/m.°C
Specific heat capacity377–379J/kg.°C
Thermal expansion coefficient18.9–20.1µstrain/°C
Thermal shock resistance53.4–60.2°C
Thermal distortion resistance5.97–6.45MW/m
Latent heat of fusion220–240kJ/kg

CuZn34Pb1 Electrical properties

Electrical resistivity6.46–6.92µohm.cm
Electrical conductivity24.9–26.7%IACS
Galvanic potential-0.33–-0.25V

CuZn34Pb1 Magnetic properties

Magnetic typeNon-magnetic

CuZn34Pb1 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3480–3590m/s
Mechanical loss coefficient (tan delta)2.78e-4–3.31e-4 

CuZn34Pb1 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingLimited use
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed79.2 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor

CuZn34Pb1 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn34Pb1 C34000 Soft Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn34Pb1 Notes

CuZn34Pb1 C34000 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn34Pb1 Standards with similar compositions

Canada: HC.4.ZP341 to CSA HC.4.3
Denmark: 5140 to DS 3003
Europe: CW600N to CEN EN 12164, CW600N to CEN EN 12166, CW600N to CEN EN 12167, CW600N to CEN EN 12449, CW600N to CEN EN 1652
Finland: CuZn36Pb1 to SFS 2923
International: CuZn36Pb1 to ISO 1634, CuZn36Pb1 to ISO 1637, CuZn36Pb1 to ISO 1638, CuZn36Pb1 to ISO 426-2
Norway: 16150 to NS 16150
South Africa: Cu-Zn36Pb1 to SABS 460
UK: CZ118 to BS 2870
USA: 65Cu-34Zn-1Pb to QQ B-613, 65Cu-34Zn-1Pb to QQ B-626, C34000, C34000 to ASTM B121/B121M, C34000 to ASTM B453M, C34000 to CDA Datasheet, C35000 to SAE J463, UNS C34000, UNS C34700
Tradenames: BOHNALLOY R64, BOHNOLLOY R65, DELTA TR4 HIGH SPEED MACHINING ROD, IMI 410, MEDIUM LEADED BRASS 229, MEDIUM LEADED BRASS-340, MUELLER 3470, NITTANY NO. 30, NITTANY NO. 35, NORANDA 3400, REVERE ALLOY NO. 340, REVERE NO. 234, RM 421, SCOVILL MATRIX BRASS 340, SVENSKA SM-1263, TITAN NO. 35, WESTERN ALLOY NO. 62, WESTERN MEDIUM LEADED BRASS #62, WIELAND-Z11