CuZn33 (C26800) Yellow Brass, Soft Material Data Sheet

CuZn33 (C26800) Yellow Brass Material Data Sheet (Wrought, Soft)

CuZn33 C26800 Soft Overview

CuZn33 C26800 soft is a wrought brass (UNS C26800), known as yellow brass. Condition: Soft. This CuZn33 C26800 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn33 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn33 brass parts in-house and inspects them before shipment.

CuZn33 Designation

CuZn33, wrought
ConditionSoft
UNS numberC26800
EN nameCW506L
ISO nameCuZn33
JIS (Japanese) nameC2680

CuZn33 C26800 Soft Composition detail

Cu (copper)63.8–68.7%
Fe (iron)0–0.05%
Pb (lead)0–0.15%
Zn (zinc)31.3–36%

CuZn33 Physical properties

Density8.38–8.55g/cm3

CuZn33 C26800 Soft Mechanical properties

Young’s modulus99.9–106GPa
Specific stiffness11.8–12.5MN.m/kg
Yield strength (elastic limit)120–130MPa
Tensile strength325–340MPa
Specific strength14.2–15.4kN.m/kg
Elongation56–58% strain
Compressive strength120–130MPa
Flexural modulus99.9–106GPa
Flexural strength (modulus of rupture)120–130MPa
Shear modulus37–39.2GPa
Bulk modulus108–115GPa
Poisson’s ratio0.34–0.35 
Shape factor29
Hardness – Vickers64–75HV
Elastic stored energy (springs)69.7–82.4kJ/m3
Fatigue strength at 10^7 cycles155–159MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
150–165MPa

CuZn33 Impact & fracture properties

Fracture toughness67.9–70.4MPa.m0.5
Toughness (G)44.4–48.6kJ/m2

CuZn33 C26800 Soft Thermal properties

Melting point927–942°C
Maximum service temperature200–210°C
Minimum service temperature-273  °C
Thermal conductivity118–124W/m.°C
Specific heat capacity378–380J/kg.°C
Thermal expansion coefficient18.9–20.1µstrain/°C
Thermal shock resistance58.8–66°C
Thermal distortion resistance5.97–6.45MW/m
Latent heat of fusion220–240kJ/kg

CuZn33 Electrical properties

Electrical resistivity6.17–6.61µohm.cm
Electrical conductivity26.1–27.9%IACS
Galvanic potential-0.32–-0.24V

CuZn33 Magnetic properties

Magnetic typeNon-magnetic

CuZn33 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3430–3540m/s
Mechanical loss coefficient (tan delta)2.37e-4–2.78e-4 

CuZn33 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingExcellent
Metal press formingAcceptable
Metal deep drawingAcceptable
Machining speed57.9 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor

CuZn33 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn33 C26800 Soft Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn33 Notes

CuZn33 C26800 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn33 Standards with similar compositions

Australia: C26800 to AS 2738, C27000 to AS 2738
Canada: HC.4.Z34(268) to CSA HC.4.2
France: CuZn33 to NF A51-101, CuZn33 to NF A51-104
International: CuZn33 to ISO 1634, CuZn33 to ISO 1638, CuZn33 to ISO 426-1
Japan: C2680 P/R to JIS H3100, C2680 TW to JIS H3320, C2700 BD to JIS H3250, C2700 BE to JIS H3250, C2700 T to JIS H3300, C2700 W to JIS H3260
UK: CZ107 to BS 2870, CZ107 to BS 2873
USA: 65.5Cu-35.5Zn to AMS 4555, 65Cu-35Zn to QQ B-613, 65Cu-35Zn to QQ W-321, C26800, C26800 to ASTM B36/B36M, C26800 to ASTM B587, C26800 to SAE J463, C27000, C27000 to AMS 4712E, C27000 to ASTM B134, C27000 to ASTM B135M, C27000 to ASTM B587, C27000 to SAE J463, UNS C26800, UNS C27000
Tradenames: 2680, ANACONDA 268, ANACONDA 67, BRIDGEPORT NO. 1, COLD HEADING 4, DEGUSSA ALLOY, DIPPING BRASS, ENGLISH SPECULUM, EYELET BRASS, FEDERALOY RS-13, FUCHS 2167, HAMILTON METAL-B, IMI 233, JAPAN BRASS, LEADED TUBE BRASS 3301, MUELLER 2600, OLIN YELLOW BRASS 268, PRYM 227, REVERE ALLOY NO. 268, SCOVILL HIGH BRASS, 270, SEYMOUR 2265, SIN-CHU, SPRABRASS Y, TWO-TO-ONE, WESTERN ALLOY NO. 34, WIELAND-M33, YELLOW BRASS 59, YELLOW BRASS 66%