Home » Brass Alloys » CuZn30 (C43600) Arsenical 70/30 Brass, Hard Material Data Sheet
CuZn30 (C43600) Arsenical 70/30 Brass, Hard Material Data Sheet
CuZn30 (C43600) Arsenical 70/30 Brass Material Data Sheet (Wrought, Hard)
CuZn30 C43600 Hard Overview
CuZn30 C43600 hard is a wrought brass (UNS C43600), known as arsenical 70/30 brass. Condition: Hard. This CuZn30 C43600 hard material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn30 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn30 brass parts in-house and inspects them before shipment.
CuZn30 Designation
CuZn30, wrought
Condition
Hard
EN name
CW701R
ISO name
CuZn19Sn
JIS (Japanese) name
C4350
CuZn30 Typical uses
Standard for condenser tubes, the arsenic inhibits dezincification.
CuZn30 C43600 Hard Composition detail
As (arsenic)
0
–
0.06
%
Cu (copper)
69.9
%
Zn (zinc)
30
%
CuZn30 Physical properties
Density
8.38
–
8.55
g/cm3
CuZn30 C43600 Hard Mechanical properties
Young’s modulus
102
–
108
GPa
Specific stiffness
12
–
12.8
MN.m/kg
Yield strength (elastic limit)
380
–
460
MPa
Tensile strength
465
–
505
MPa
Specific strength
44.9
–
54.4
kN.m/kg
Elongation
10
–
20
% strain
Compressive strength
380
–
460
MPa
Flexural modulus
102
–
108
GPa
Flexural strength (modulus of rupture)
380
–
460
MPa
Shear modulus
37.7
–
40
GPa
Bulk modulus
110
–
117
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
19
Hardness – Vickers
165
–
180
HV
Elastic stored energy (springs)
692
–
1000
kJ/m3
Fatigue strength at 10^7 cycles
195
–
206
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
181
–
222
MPa
CuZn30 Impact & fracture properties
Fracture toughness
31.1
–
35.8
MPa.m0.5
Toughness (G)
9.24
–
12.2
kJ/m2
CuZn30 C43600 Hard Thermal properties
Melting point
952
–
967
°C
Maximum service temperature
180
–
190
°C
Minimum service temperature
-200
°C
Thermal conductivity
118
–
124
W/m.°C
Specific heat capacity
378
–
380
J/kg.°C
Thermal expansion coefficient
18.4
–
19.6
µstrain/°C
Thermal shock resistance
189
–
233
°C
Thermal distortion resistance
6.12
–
6.63
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn30 Electrical properties
Electrical resistivity
7.94
–
8.51
µohm.cm
Electrical conductivity
20.3
–
21.7
%IACS
Temperature dependence of resistivity
2.5
–
3.5
/°C
Galvanic potential
-0.3
–
-0.22
V
CuZn30 Magnetic properties
Magnetic type
Non-magnetic
CuZn30 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3470
–
3580
m/s
Mechanical loss coefficient (tan delta)
1.9e-5
–
2.8e-5
CuZn30 Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Excellent
Metal press forming
Acceptable
Metal deep drawing
Limited use
Machining speed
57.9 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Poor
CuZn30 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuZn30 C43600 Hard Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible
CuZn30 Notes
CuZn30 C43600 Hard Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn30 Standards with similar compositions
Australia: 259 to AS 1567, 259 to AS 1572, C26130 to AS 2738