CuZn27Al4.5 High-Tensile Brass Material Data Sheet (Wrought, As Drawn)
CuZn27Al4.5 As Drawn Brass Overview
CuZn27Al4.5 as drawn brass is a wrought brass (CZ116), known as high-tensile brass. Condition: As drawn. This CuZn27Al4.5 as drawn brass material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn27Al4.5 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn27Al4.5 brass parts in-house and inspects them before shipment.
CuZn27Al4.5 Designation
CuZn27Al4.5, wrought Condition As drawn EN name CZ116 Tradenames HT27
CuZn27Al4.5 Typical uses
Architectural sections, fixings, forgings, pump parts, pressure tubes.
CuZn27Al4.5 As Drawn Brass Composition detail
Al (aluminum) 4 – 5 % Cu (copper) 64 – 68 % Fe (iron) 0.25 – 1.2 % Mn (manganese) 0.3 – 2 % Zn (zinc) 23.3 – 31.4 % Other 0 – 0.5 %
CuZn27Al4.5 Physical properties
CuZn27Al4.5 As Drawn Brass Mechanical properties
Young’s modulus 101 – 107 GPa Specific stiffness 12.1 – 12.9 MN.m/kg Yield strength (elastic limit) 290 – 310 MPa Tensile strength 540 – 570 MPa Specific strength 34.8 – 37.3 kN.m/kg Elongation 12 – 15 % strain Compressive strength 290 – 310 MPa Flexural modulus 101 – 107 GPa Flexural strength (modulus of rupture) 290 – 310 MPa Shear modulus 37.4 – 39.6 GPa Bulk modulus 109 – 116 GPa Poisson’s ratio 0.34 – 0.35 Shape factor 24 Hardness – Vickers 165 – 170 HV Elastic stored energy (springs) 403 – 464 kJ/m3 Fatigue strength at 10^7 cycles 215 – 223 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 206 – 232 MPa
CuZn27Al4.5 Impact & fracture properties
Fracture toughness 41.3 – 43.2 MPa.m0.5 Toughness (G) 16.3 – 18.1 kJ/m2
CuZn27Al4.5 As Drawn Brass Thermal properties
Melting point 952 – 967 °C Maximum service temperature 180 – 190 °C Minimum service temperature -170 – -160 °C Thermal conductivity 110 – 117 W/m.°C Specific heat capacity 377 – 379 J/kg.°C Thermal expansion coefficient 18.9 – 20.1 µstrain/°C Thermal shock resistance 140 – 156 °C Thermal distortion resistance 5.57 – 6.08 MW/m Latent heat of fusion 220 – 240 kJ/kg
CuZn27Al4.5 Electrical properties
Electrical resistivity 7.59 – 8.13 µohm.cm Electrical conductivity 21.2 – 22.7 %IACS Temperature dependence of resistivity 2.5 – 3.5 /°C Galvanic potential -0.34 – -0.26 V
CuZn27Al4.5 Magnetic properties
Magnetic type Non-magnetic
CuZn27Al4.5 Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 3480 – 3590 m/s Mechanical loss coefficient (tan delta) 4.2e-5 – 4.8e-5
CuZn27Al4.5 Processing properties
Metal casting Unsuitable Metal cold forming Acceptable Metal hot forming Acceptable Metal press forming Acceptable Metal deep drawing Limited use Machining speed 54.9 m/min Weldability Notes: Preheating and post weld heat treatments are required Good
CuZn27Al4.5 Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Acceptable Strong acids Unacceptable Weak alkalis Excellent Strong alkalis Excellent Organic solvents Excellent Oxidation at 500C Limited use UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Excellent Flammability Non-flammable
CuZn27Al4.5 As Drawn Brass Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide Highly susceptible
CuZn27Al4.5 Notes
CuZn27Al4.5 As Drawn Other notes (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn27Al4.5 Standards with similar compositions
UK: CZ116 to BS 2872, CZ116 to BS 2874Tradenames: CERRO HT27, DELTA HT17, DELTA HT27, MCKECHNIE 65