CuZn20 (C24000) Low Brass, Soft Material Data Sheet

CuZn20 (C24000) Low Brass Material Data Sheet (Wrought, Soft)

CuZn20 C24000 Soft Overview

CuZn20 C24000 soft is a wrought brass (UNS C24000), known as low brass. Condition: Soft. This CuZn20 C24000 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn20 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn20 brass parts in-house and inspects them before shipment.

CuZn20 Designation

CuZn20, wrought
ConditionSoft
UNS numberC24000
EN nameCW503L
ISO nameCuZn20
GB (Chinese) nameH80
JIS (Japanese) nameC2400

CuZn20 Typical uses

Architectural & decorative items, jewelry, enameled & brazed parts.

CuZn20 C24000 Soft Composition detail

Cu (copper)78.4–81.6%
Fe (iron)0–0.05%
Pb (lead)0–0.05%
Zn (zinc)18.4–21.5%

CuZn20 Physical properties

Density8.53–8.7g/cm3

CuZn20 C24000 Soft Mechanical properties

Young’s modulus112–118GPa
Specific stiffness13–13.7MN.m/kg
Yield strength (elastic limit)120–140MPa
Tensile strength310–330MPa
Specific strength13.9–16.3kN.m/kg
Elongation50–52% strain
Compressive strength120–140MPa
Flexural modulus112–118GPa
Flexural strength (modulus of rupture)120–140MPa
Shear modulus41.4–43.7GPa
Bulk modulus121–127GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers63–72HV
Elastic stored energy (springs)62.9–84.9kJ/m3
Fatigue strength at 10^7 cycles150–156MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
143–163MPa

CuZn20 Impact & fracture properties

Fracture toughness65.5–70.4MPa.m0.5
Toughness (G)37.2–43.2kJ/m2

CuZn20 C24000 Soft Thermal properties

Melting point982–997°C
Maximum service temperature200–210°C
Minimum service temperature-273  °C
Thermal conductivity135–140W/m.°C
Specific heat capacity380–382J/kg.°C
Thermal expansion coefficient17.5–18.5µstrain/°C
Thermal shock resistance57.5–68.2°C
Thermal distortion resistance7.39–7.9MW/m
Latent heat of fusion220–240kJ/kg

CuZn20 Electrical properties

Electrical resistivity5.25–5.62µohm.cm
Electrical conductivity30.7–32.8%IACS
Galvanic potential-0.27–-0.19V

CuZn20 Magnetic properties

Magnetic typeNon-magnetic

CuZn20 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3600–3710m/s
Mechanical loss coefficient (tan delta)2.04e-4–2.78e-4 

CuZn20 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingLimited use
Metal press formingAcceptable
Metal deep drawingAcceptable
Machining speed48.8 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good

CuZn20 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn20 C24000 Soft Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn20 Notes

CuZn20 C24000 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn20 Standards with similar compositions

Australia: C24000 to AS 2738
Canada: HC.4.Z20(240) to CSA HC.4.2
Czech Republic: CuZn20 to CSN 423203
Denmark: 5114 to DS 3003
Finland: CuZn20 to SFS 2917
France: CuZn20 to NF A51-101, CuZn20 to NF A51-104
Germany: 2.025 to DIN, CuZn20 to DIN
International: CuZn20 to ISO 1634, CuZn20 to ISO 1638, CuZn20 to ISO 426-1
Japan: C2400 P/R to JIS H3100, C2400 W to JIS H3260
Norway: 16110 to NS 16110
Sweden: 5114-02 to SIS 145114, 5114-04 to SIS 145114, 5114-05 to SIS 145114
UK: CZ103 to BS 2870, CZ103 to BS 2873, CZ103 to BS 2874
USA: 80Cu-20Zn to QQ B-613, 80Cu-20Zn to QQ B-626, 80Cu-20Zn to QQ B-650, 80Cu-20Zn to QQ W-321, C24000, C24000 to ASTM B134, C24000 to ASTM B36/B36M, C24000 to SAE J463, C24080, UNS C24000, UNS C24080
Tradenames: 2400, 80/20 LOW BRASS, ANSONIA ALLOY C24000, ARKO, BOLTOMET 516, BRIDGEPORT NO. 5, CERRO CF9, FUCHS 2180, IMI 220, LOW BRASS, LOW BRASS 5, MCKECHNIE 310, MESSING 80, OLIN LOW BRASS 240, OUTOKUMPU MS80, PRYM 224, RED BRASS, REVERE LOW BRASS, REVERE NO. 240, RIVERSIDE 66, RM 220, SCOVILL LOW BRASS, ALLOY 240, SEYMOUR 2280, SEYMOUR 280, SM-1080, TOMBAC-A, VOLCO NO. 80, WESTERN LOW BRASS 20, WIELAND-M20