CuZn15 (C23000) Red Brass, Soft Material Data Sheet

CuZn15 (C23000) Red Brass Material Data Sheet (Wrought, Soft)

CuZn15 C23000 Soft Overview

CuZn15 C23000 soft is a wrought brass (UNS C23000), known as red brass. Condition: Soft. This CuZn15 C23000 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn15 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn15 brass parts in-house and inspects them before shipment.

CuZn15 Designation

CuZn15, wrought
ConditionSoft
UNS numberC23000
EN nameCW502L
ISO nameCuZn15
GB (Chinese) nameH85
JIS (Japanese) nameC2300

CuZn15 Typical uses

Architectural & decorative items, jewelry, enameled & brazed parts.

CuZn15 C23000 Soft Composition detail

Cu (copper)84–86%
Fe (iron)0–0.05%
Pb (lead)0–0.05%
Zn (zinc)13.9–16%

CuZn15 Physical properties

Density8.58–8.75g/cm3

CuZn15 C23000 Soft Mechanical properties

Young’s modulus114–122GPa
Specific stiffness13.1–14.1MN.m/kg
Yield strength (elastic limit)120–130MPa
Tensile strength295–310MPa
Specific strength13.8–15kN.m/kg
Elongation38–40% strain
Compressive strength120–130MPa
Flexural modulus114–122GPa
Flexural strength (modulus of rupture)120–130MPa
Shear modulus42.2–45.1GPa
Bulk modulus123–132GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers63–68HV
Elastic stored energy (springs)60.8–72kJ/m3
Fatigue strength at 10^7 cycles145–150MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
140–155MPa

CuZn15 Impact & fracture properties

Fracture toughness67.9–70.4MPa.m0.5
Toughness (G)38.6–42.6kJ/m2

CuZn15 C23000 Soft Thermal properties

Melting point1010–1020°C
Maximum service temperature200–210°C
Minimum service temperature-273  °C
Thermal conductivity156–161W/m.°C
Specific heat capacity381–383J/kg.°C
Thermal expansion coefficient17–18µstrain/°C
Thermal shock resistance57.1–64.2°C
Thermal distortion resistance8.77–9.36MW/m
Latent heat of fusion220–240kJ/kg

CuZn15 Electrical properties

Electrical resistivity4.47–4.79µohm.cm
Electrical conductivity36–38.6%IACS
Galvanic potential-0.25–-0.17V

CuZn15 Magnetic properties

Magnetic typeNon-magnetic

CuZn15 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3620–3760m/s
Mechanical loss coefficient (tan delta)2.37e-4–2.78e-4 

CuZn15 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingLimited use
Metal press formingAcceptable
Metal deep drawingAcceptable
Machining speed45.7 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good

CuZn15 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsAcceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn15 C23000 Soft Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Susceptible

CuZn15 Notes

CuZn15 C23000 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn15 Standards with similar compositions

Australia: 230 to AS 1566, C23000 to AS 2738
Canada: HC.4.Z15(230) to CSA HC.4.2
Czech Republic: CuZn15 to CSN 423202
Denmark: 5112 to DS 3003
Finland: CuZn15 to SFS 2916
France: CuZn15 to NF A51-101, CuZn15 to NF A51-104
Germany: 2.024 to DIN, CuZn15 to DIN
International: CuZn15 to ISO 1634, CuZn15 to ISO 1635, CuZn15 to ISO 1637, CuZn15 to ISO 1638, CuZn15 to ISO 426-1
Japan: C2300 P/R to JIS H3100, C2300 to JIS H3300, C2300 W to JIS H3260
Norway: 16108 to NS 16108
Sweden: 5112-02 to SIS 145112, 5112-04 to SIS 145112, 5112-05 to SIS 145112
UK: CZ102 to BS 2870, CZ102 to BS 2873
USA: 85Cu-15Zn to MIL T-20168, 85Cu-15Zn to QQ B-613, 85Cu-15Zn to QQ B-626, 85Cu-15Zn to QQ W-321, C23000, C23000 to ASTM B111M, C23000 to ASTM B134, C23000 to ASTM B135M, C23000 to ASTM B359M, C23000 to ASTM B36/B36M, C23000 to ASTM B395M, C23000 to ASTM B43, C23000 to ASTM B543M, C23000 to ASTM B569, C23000 to ASTM B587, C23000 to ASTM B888, C23000 to SAE J463, UNS C23000
Tradenames: 2300, 85/15 RICH LOW BRASS, ANACONDA 230, ANACONDA 85, BOLTOMET 514, BRAZING METAL F, BRIDGEPORT NO. 85, FUCHS 2185, IMI 215, MESSING 85, MUELLER 2300, OLIN RED BRASS, OUTOKUMPU MS85, PLUMRITE 85, PLUMRITE STANDARD 85, PRINCES METAL NO. 2, PRYM 223, RED BRASS, RED BRASS 230, RED BRASS, 85%, REVERE RED BRASS, RIVERSIDE 62, RM 215, SCOVILL RED BRASS, 85%, ALLOY 230, SEYMOUR 2285, SEYMOUR 285, SM-1085, TOMBAC, OKER, VOLCO NO. 10, WESTERN ALLOY NO. 15, WESTERN RED BRASS #15, WIELAND-M15, WOLVERINE ALLOY 28