AISI 204-Cu Stainless steel, Annealed, Austenitic | Designation | Equivalent Grades & Similar Grades  

AISI 204-Cu Stainless steel-1.4597-X9CrMnCuNB17-8-3, S20430 Designation Equivalent Modulus Metal Turkey Turkiye

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | Foundry | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding |Turkiye

Designation: Type 204-Cu, wrought

UNS number S20430
US name AISI 204-Cu
EN name X9CrMnCuNB17-8-3
EN number 1.4597
CountryEquivalent / Similar Grade
USAS20430 to ASTM A313/A313M, S20430 to ASTM A959, UNS S20430
Tradenames:CARPENTER TYPE 204-CU STAINLESS

AISI 201 Stainless steel (Low nickel work hardenable), austenitic, 3/4 hard | Toughness | Fracture Toughness

AISI 201 stainless steel 3-4 Hard Fracture Toughness, Modulus Metal,Turkey,Turkiye.

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | Foundry | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding |Turkiye

Fracture Toughness & ToughnessValues
Fracture toughness* 72 – 81 MPa.m^0.5
Toughness (G)* 26.4 – 33.3 kJ/m^2
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.



AISI 201 Stainless steel (Low nickel work hardenable), austenitic, Annealed | Toughness | Fracture Toughness

AISI 201 stainless steel Annealed Fracture Toughness, Modulus Metal,Turkey,Turkiye.

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | Foundry | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding |Turkiye

Fracture Toughness & ToughnessValues
Fracture toughness60 – 75 MPa.m^0.5
Toughness (G)18.5 – 28.3 kJ/m^2
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.



AISI 201 Stainless steel (Low nickel work hardenable), austenitic, Full Hard | Toughness | Fracture Toughness

AISI 201 stainless steel Full Hard Fracture Toughness, Modulus Metal,Turkey,Turkiye.

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | Foundry | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding |Turkiye

Fracture Toughness & ToughnessValues
Fracture toughness*73 – 82 MPa.m^0.5
Toughness (G)*27.1 – 34.1 kJ/m^2
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.



AISI 201L Stainless steel (Low nickel work hardenable), austenitic, Annealed | Toughness | Fracture Toughness

AISI 201L stainless steel Annealed Fracture Toughness, Modulus Metal,Turkey,Turkiye

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | Foundry | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding |Turkiye

Fracture Toughness & ToughnessValues
Fracture toughness60 – 75 MPa.m^0.5
Toughness (G)18.5 – 28.3 kJ/m^2
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.



AISI 201LN Stainless steel (Low nickel work hardenable), austenitic, Annealed | Toughness | Fracture Toughness

AISI 201LN stainless steel Annealed Fracture Toughness, Modulus Metal,Turkey,Turkiye.

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | Foundry | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding |Turkiye

Fracture Toughness & ToughnessValues
Fracture toughness*60.8 – 74.3 MPa.m^0.5
Toughness (G)*18.9 – 27.8 kJ/m^2
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.


AISI 202 Stainless steel (Low nickel general purpose), austenitic, 1/2 hard | Toughness | Fracture Toughness

AISI 202 Stainless Steel 1-2 Hard Fracture Toughness, Modulus Metal Turkey, Turkiye

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | Foundry | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding |Turkiye

Fracture Toughness & ToughnessValues
Fracture toughness* 65 – 99 MPa.m^0.5
Toughness (G)* 21.9 – 47.4 kJ/m^2
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.

AISI 202 Stainless steel (Low nickel general purpose), austenitic, 1/4 hard | Toughness | Fracture Toughness

AISI 202 Stainless Steel 1-4 Hard Fracture Toughness, Modulus Metal Turkey, Turkiye

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | Foundry | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding |Turkiye

Fracture Toughness & ToughnessValues
Fracture toughness* 70 – 137 MPa.m^0.5
Toughness (G)* 26.7 – 86.4 kJ/m^2
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.

AISI 202 Stainless steel (Low nickel general purpose), austenitic, Annealed | Toughness | Fracture Toughness

AISI 202 Stainless Steel Annealed Fracture Toughness, Modulus Metal Turkey, Turkiye

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | Foundry | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding |Turkiye

Fracture Toughness & ToughnessValues
Fracture toughness 60 – 75 MPa.m^0.5
Toughness (G)* 18.1 – 28 kJ/m^2
*Values indicated with asterisks (*) are approximate. No guarantee is provided for

AISI 201 Stainless steel (Low nickel work hardenable), austenitic, 1/2 hard | Toughness | Fracture Toughness

AISI 201 stainless steel 1-2 Hard Fracture Toughness, Modulus Metal,Turkey,Turkiye

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | Foundry | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding |Turkiye

Fracture Toughness & ToughnessValues
Fracture toughness* 65 – 100 MPa.m^0.5
Toughness (G)* 22.3 – 48.9 kJ/m^2
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.