Welded structures, pressure vessels, tube for marine service
Aluminum 5454 Composition detail
Al (aluminum)
94.4
–
97
%
Cr (chromium)
0.05
–
0.2
%
Cu (copper)
0
–
0.1
%
Fe (iron)
0
–
0.4
%
Mg (magnesium)
2.4
–
3
%
Mn (manganese)
0.5
–
1
%
Si (silicon)
0
–
0.25
%
Ti (titanium)
0
–
0.2
%
Zn (zinc)
0
–
0.25
%
Other
0
–
0.15
%
Aluminum 5454 Physical properties
Density
2.67
–
2.7
g/cm3
Aluminum 5454 Mechanical properties
Young’s modulus
70
–
73.6
GPa
Specific stiffness
26.1
–
27.4
MN.m/kg
Yield strength (elastic limit)
83
–
91.7
MPa
Tensile strength
214
–
237
MPa
Specific strength
30.9
–
34.2
kN.m/kg
Elongation
12
–
18
% strain
Compressive strength
83
–
91.7
MPa
Flexural modulus
70
–
73.6
GPa
Flexural strength (modulus of rupture)
83
–
91.7
MPa
Shear modulus
27
–
28.4
GPa
Bulk modulus
69
–
72.5
GPa
Poisson’s ratio
0.33
–
0.343
Shape factor
41
Hardness – Vickers
57
–
63
HV
Elastic stored energy (springs)
48
–
58.7
kJ/m3
Fatigue strength at 10^7 cycles
118
–
130
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
110
–
139
MPa
Aluminum 5454 Impact & fracture properties
Fracture toughness
34
–
36
MPa.m0.5
Toughness (G)
16
–
18.1
kJ/m2
Aluminum 5454 Thermal properties
Melting point
600
–
645
°C
Maximum service temperature
150
–
170
°C
Minimum service temperature
-273
°C
Thermal conductivity
135
–
146
W/m.°C
Specific heat capacity
963
–
1e3
J/kg.°C
Thermal expansion coefficient
23.6
–
24.8
µstrain/°C
Thermal shock resistance
47.3
–
53.4
°C
Thermal distortion resistance
5.55
–
6.09
MW/m
Latent heat of fusion
384
–
393
kJ/kg
Aluminum 5454 Electrical properties
Electrical resistivity
5
–
5.2
µohm.cm
Electrical conductivity
33.2
–
34.5
%IACS
Galvanic potential
-0.81
–
-0.73
V
Aluminum 5454 Magnetic properties
Magnetic type
Non-magnetic
Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5100
–
5240
m/s
Mechanical loss coefficient (tan delta)
1e-4
–
0.002
Aluminum 5454 Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Acceptable
Metal press forming
Acceptable
Metal deep drawing
Limited use
Machining speed
171 m/min
Weldability Notes: Preheating and post weld heat treatments are not required
Good
Aluminum 5454 Durability
Water (fresh)
Excellent
Water (salt)
Acceptable
Weak acids
Excellent
Strong acids
Excellent
Weak alkalis
Acceptable
Strong alkalis
Unacceptable
Organic solvents
Excellent
Oxidation at 500C
Unacceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Aluminum alloys perform poorly when self-mated but can be processed without galling when mated with steels.
Limited use
Flammability
Non-flammable
Aluminum 5454 Corrosion resistance of metals
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Halide, water
Slightly susceptible
Aluminum 5454 Standards with similar compositions
Australia: 5454 to AS 2848.1
Canada: GM31N to CSA
Europe: EN AW-5454 to CEN EN 573-3, EN AW-5554 to CEN EN 573-3
France: 5454 to NF A50-411
Germany: 3.3537/AlMg2.7Mn to DIN 1725-1, 3.3538 to DIN 1732-1, SG-AlMg2.7Mn to DIN 1732-1
Hungary: H-AlMg2.5Mn to MSZ 4264
International: AlMg3Mn to ISO 209-1, AlMg3Mn(A) to ISO 209-1
Japan: A5454P to JIS H4000, A5454S to JIS H4100, A5454TE to JIS H4080
Norway: 17212 to NS 17212
South Africa: 54540(Al-Mg3Mn) to SABS 712
UK: 5454 to BS 1470, 5454 to BS 4300/10
USA: 5354, 5454, 5454 to ASTM B209M, 5454 to ASTM B221M, 5454 to ASTM B234, 5454 to ASTM B241M, 5454 to ASTM B404/B404M, 5454 to ASTM B547/B547M, 5454 to QQ A-250/10, 5554, ER5554 to AWS A5.10/A5.10M, R5554 to AWS A5.10/A5.10M, UNS A95454, UNS A95554