CuSn4 C51000 Hard Overview
CuSn4 C51000 hard is a wrought bronze (UNS C51000, EN CW451K), known as 5% phosphor bronze. Condition: Hard. This CuSn4 C51000 hard material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C51000 bronze parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C51000 bronze parts in-house and inspects them before shipment.
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
235
–
243
MPa
C51000 Impact & fracture properties
Fracture toughness
28.8
–
29.2
MPa.m0.5
Toughness (G)
7.15
–
7.42
kJ/m2
CuSn4 C51000 Hard Thermal properties
Melting point
932
–
1060
°C
Maximum service temperature
150
–
160
°C
Minimum service temperature
-273
°C
Thermal conductivity
74
–
76
W/m.°C
Specific heat capacity
384
–
385
J/kg.°C
Thermal expansion coefficient
16.5
–
17.5
µstrain/°C
Thermal shock resistance
249
–
266
°C
Thermal distortion resistance
4.27
–
4.56
MW/m
Latent heat of fusion
220
–
240
kJ/kg
C51000 Electrical properties
Electrical resistivity
13.5
–
15.1
µohm.cm
Electrical conductivity
11.4
–
12.8
%IACS
Temperature dependence of resistivity
2
–
2.5
/°C
Galvanic potential
-0.22
–
-0.14
V
C51000 Magnetic properties
Magnetic type
Non-magnetic
C51000 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3620
–
3660
m/s
Mechanical loss coefficient (tan delta)
1.5e-5
–
1.6e-5
C51000 Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Limited use
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
33.5 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
C51000 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuSn4 C51000 Hard Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible
C51000 Notes
CuSn4 C51000 Hard Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C51000 Standards with similar compositions
Australia: 518 to AS 1566, 518 to AS 1567, C51000 to AS 2738, C51800 to AS 2738
Europe: CW451K to CEN EN 12163, CW451K to CEN EN 12166, CW451K to CEN EN 1652, CW451K to CEN EN 1654
UK: C10 to BS 2901/3, PB102 to BS 2870, PB102 to BS 2873, PB102 to BS 2874, PB102 to BS 2875
USA: 94.8Cu-5Sn-.2P to MIL B-13501, 94.8Cu-5Sn-.2P to QQ B-750, 94.8Cu-5Sn-.2P to QQ W-321, 94Cu-5.0Sn-0.19P to AMS 4720, 95Cu-5Sn to AMS 4625, C51000, C51000 to ASTM B100, C51000 to ASTM B103/B103M, C51000 to ASTM B139M, C51000 to ASTM B159M, C51000 to ASTM B888, C51800, ECuSn-A to AWS A5.6, ERCuSn-A to AWS A5.7, UNS C51000, UNS C51800
Tradenames: 5100, ANACONDA (A) 510, BOLTON NO. 10 PHOSPHOR BRONZE, BRUSH PHOSPHOR BRONZE, LUVATA C510, MILLER 200PLUS GR. A, OLIN PHOSPHOR BRONZE, 5%, PHOS. BRONZE, PHOSPHOR 36 BRONZE GRADE A, PHOSPHOR BRONZE 5% A 510, PHOSPHOR BRONZE A510, PHOSPHOR BRONZE GRADE A, PHOSPHOR BRONZE NO. 30, REVERE ALLOY NO. 310, SEYMOUR 9950, SEYMOUR NO. 9522, WESTERN PHOSPHOR BRONZE 5%, #106, ZEPHOR BRONZE