Home » Bronze Alloys » C93500 Leaded Bronze 85-5-10, Cast Material Data Sheet
C93500 Leaded Bronze 85-5-10, Cast Material Data Sheet
C93500 Leaded Bronze 85-5-10 Material Data Sheet (Cast)
C93500 Cast Bronze Overview
C93500 cast bronze is a cast bronze (UNS C93500), known as leaded bronze 85-5-10. Condition: Cast. This C93500 cast bronze material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C93500 bronze castings from Turkey (Türkiye)? Modulus Metal supplies C93500 bronze castings with in-house CNC machining and inspects them before shipment.
C93500 Designation
Copper Alloy: CuSn5Pb10 (UNS C93500)
UNS number
C93500
C93500 Typical uses
Bearings and bushes to resist corrosion and poor lubrication (plasticity increases with lead content, making them suitable for minor misalignment and for use with soft steel shafts).
C93500 Cast Bronze Composition detail
Al (aluminum)
0
–
0.005
%
Cu (copper)
80.4
–
87.7
%
Fe (iron)
0
–
0.2
%
Ni (nickel)
0
–
1
%
P (phosphorus)
0
–
0.05
%
Pb (lead)
8
–
10
%
S (sulfur)
0
–
0.08
%
Sb (antimony)
0
–
0.3
%
Si (silicon)
0
–
0.005
%
Sn (tin)
4.3
–
6
%
Zn (zinc)
0
–
2
%
C93500 Physical properties
Density
8.91
–
9.09
g/cm3
C93500 Cast Bronze Mechanical properties
Young’s modulus
72
–
74
GPa
Specific stiffness
7.97
–
8.25
MN.m/kg
Yield strength (elastic limit)
60
–
130
MPa
Tensile strength
160
–
230
MPa
Specific strength
6.67
–
14.4
kN.m/kg
Elongation
5
–
9
% strain
Compressive strength
60
–
130
MPa
Flexural modulus
72
–
74
GPa
Flexural strength (modulus of rupture)
60
–
130
MPa
Shear modulus
26.6
–
27.4
GPa
Bulk modulus
77.8
–
79.9
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
29
Hardness – Vickers
55
–
75
HV
Hardness – Brinell
55
–
80
HB
Elastic stored energy (springs)
27.5
–
104
kJ/m3
Fatigue strength at 10^7 cycles
90
–
100
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
67.6
–
133
MPa
C93500 Impact & fracture properties
Fracture toughness
76
–
90.5
MPa.m0.5
Toughness (G)
79.7
–
111
kJ/m2
C93500 Cast Bronze Thermal properties
Melting point
927
–
1060
°C
Maximum service temperature
180
–
190
°C
Minimum service temperature
-273
°C
Thermal conductivity
68
–
74
W/m.°C
Specific heat capacity
376
–
392
J/kg.°C
Thermal expansion coefficient
18
–
19
µstrain/°C
Thermal shock resistance
44.4
–
96.4
°C
Thermal distortion resistance
3.65
–
4.03
MW/m
Latent heat of fusion
220
–
240
kJ/kg
C93500 Electrical properties
Electrical resistivity
11
–
12
µohm.cm
Electrical conductivity
14.4
–
15.7
%IACS
Galvanic potential
-0.25
–
-0.17
V
C93500 Magnetic properties
Magnetic type
Non-magnetic
C93500 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2820
–
2870
m/s
Mechanical loss coefficient (tan delta)
4e-4
–
0.00111
C93500 Processing properties
Metal casting
Excellent
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
91.4 m/min
Weldability
Unsuitable
C93500 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Contains lead which lubricates, improving resistance.
Excellent
Flammability
Non-flammable
C93500 Cast Bronze Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible
C93500 Notes
C93500 Cast Bronze Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C93500 Standards with similar compositions
Australia: C93500 to AS 2738
Europe: CB494K to CEN EN 1982, CC494K to CEN EN 1982
International: CuPb9Sn5 to ISO 4382-1
USA: C93500, C93500 to ASTM B271, C93500 to ASTM B30, C93500 to ASTM B505, C93500 to ASTM B584, C93500 to ASTM B763, C93500 to CDA Datasheet, C93500 to SAE J462, UNS C93500