CuSn4 (C51000) 5% Phosphor Bronze, Soft Material Data Sheet

CuSn4 (C51000) 5% Phosphor Bronze Material Data Sheet (Wrought, Soft)

CuSn4 C51000 Soft Overview

CuSn4 C51000 soft is a wrought bronze (UNS C51000, EN CW451K), known as 5% phosphor bronze. Condition: Soft. This CuSn4 C51000 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C51000 bronze parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C51000 bronze parts in-house and inspects them before shipment.

C51000 Designation

CuSn4, wrought
ConditionSoft
UNS numberC51000
EN nameCW451K
ISO nameCuSn5
JIS (Japanese) nameC5102

C51000 Typical uses

Tubes & plates for condensers & acid mine waters, textile & paper-making plant, bellows, diaphragms, springs, clips, fixing components, electrical contacts, welding rods & electrodes, bearings, bourdon & pressure tubing, fuel piping.

CuSn4 C51000 Soft Composition detail

Cu (copper)93.4–95.8%
Fe (iron)0–0.1%
P (phosphorus)0.03–0.35%
Pb (lead)0–0.05%
Sn (tin)4.2–5.8%
Zn (zinc)0–0.3%

C51000 Physical properties

Density8.7–8.73g/cm3

CuSn4 C51000 Soft Mechanical properties

Young’s modulus114–117GPa
Specific stiffness13.1–13.4MN.m/kg
Yield strength (elastic limit)155–160MPa
Tensile strength335–340MPa
Specific strength17.8–18.4kN.m/kg
Elongation55–60% strain
Compressive strength155–160MPa
Flexural modulus114–117GPa
Flexural strength (modulus of rupture)155–160MPa
Shear modulus42.2–43.3GPa
Bulk modulus123–126GPa
Poisson’s ratio0.34–0.35 
Shape factor29
Hardness – Vickers70–80HV
Hardness – Brinell63–72HB
Elastic stored energy (springs)104–111kJ/m3
Fatigue strength at 10^7 cycles158–159MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
154–163MPa

C51000 Impact & fracture properties

Fracture toughness61.3–62.3MPa.m0.5
Toughness (G)32.4–33.8kJ/m2

CuSn4 C51000 Soft Thermal properties

Melting point932–1060°C
Maximum service temperature150–160°C
Minimum service temperature-273  °C
Thermal conductivity74–76W/m.°C
Specific heat capacity384–385J/kg.°C
Thermal expansion coefficient16.5–17.5µstrain/°C
Thermal shock resistance77.4–83.2°C
Thermal distortion resistance4.27–4.56MW/m
Latent heat of fusion220–240kJ/kg

C51000 Electrical properties

Electrical resistivity11.7–13.2µohm.cm
Electrical conductivity13.1–14.7%IACS
Temperature dependence of resistivity2–2.5/°C
Galvanic potential-0.22–-0.14V

C51000 Magnetic properties

Magnetic typeNon-magnetic

C51000 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3620–3660m/s
Mechanical loss coefficient (tan delta)1.56e-4–1.66e-4 

C51000 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingLimited use
Metal press formingExcellent
Metal deep drawingAcceptable
Machining speed33.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good

C51000 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuSn4 C51000 Soft Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible

C51000 Notes

CuSn4 C51000 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C51000 Standards with similar compositions

Australia: 518 to AS 1566, 518 to AS 1567, C51000 to AS 2738, C51800 to AS 2738
Europe: CW451K to CEN EN 12163, CW451K to CEN EN 12166, CW451K to CEN EN 1652, CW451K to CEN EN 1654
UK: C10 to BS 2901/3, PB102 to BS 2870, PB102 to BS 2873, PB102 to BS 2874, PB102 to BS 2875
USA: 94.8Cu-5Sn-.2P to MIL B-13501, 94.8Cu-5Sn-.2P to QQ B-750, 94.8Cu-5Sn-.2P to QQ W-321, 94Cu-5.0Sn-0.19P to AMS 4720, 95Cu-5Sn to AMS 4625, C51000, C51000 to ASTM B100, C51000 to ASTM B103/B103M, C51000 to ASTM B139M, C51000 to ASTM B159M, C51000 to ASTM B888, C51800, ECuSn-A to AWS A5.6, ERCuSn-A to AWS A5.7, UNS C51000, UNS C51800
Tradenames: 5100, ANACONDA (A) 510, BOLTON NO. 10 PHOSPHOR BRONZE, BRUSH PHOSPHOR BRONZE, LUVATA C510, MILLER 200PLUS GR. A, OLIN PHOSPHOR BRONZE, 5%, PHOS. BRONZE, PHOSPHOR 36 BRONZE GRADE A, PHOSPHOR BRONZE 5% A 510, PHOSPHOR BRONZE A510, PHOSPHOR BRONZE GRADE A, PHOSPHOR BRONZE NO. 30, REVERE ALLOY NO. 310, SEYMOUR 9950, SEYMOUR NO. 9522, WESTERN PHOSPHOR BRONZE 5%, #106, ZEPHOR BRONZE