Home » Bronze Alloys » CuSn10 (C90700) Tin Bronze, Cast Material Data Sheet
CuSn10 (C90700) Tin Bronze, Cast Material Data Sheet
CuSn10 (C90700) Tin Bronze Material Data Sheet (Cast)
CuSn10 C90700 Cast Overview
CuSn10 C90700 cast is a cast bronze (UNS C90700, EN CC480K), known as tin bronze. Condition: Cast. This CuSn10 C90700 cast material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C90700 bronze castings from Turkey (Türkiye)? Modulus Metal supplies C90700 bronze castings with in-house CNC machining and inspects them before shipment.
C90700 Designation
CuSn10
UNS number
C90700
EN name
CC480K
ISO name
CuSn10
C90700 Typical uses
General-purpose sand castings.
CuSn10 C90700 Cast Composition detail
Al (aluminum)
0
–
0.005
%
Cu (copper)
85.8
–
90
%
Fe (iron)
0
–
0.15
%
Ni (nickel)
0
–
0.5
%
P (phosphorus)
0
–
0.3
%
Pb (lead)
0
–
0.5
%
S (sulfur)
0
–
0.05
%
Sb (antimony)
0
–
0.2
%
Si (silicon)
0
–
0.005
%
Sn (tin)
10
–
12
%
Zn (zinc)
0
–
0.5
%
C90700 Physical properties
Density
8.8
–
8.82
g/cm3
CuSn10 C90700 Cast Mechanical properties
Young’s modulus
78
–
82
GPa
Specific stiffness
8.85
–
9.31
MN.m/kg
Yield strength (elastic limit)
130
–
160
MPa
Tensile strength
230
–
310
MPa
Specific strength
14.8
–
18.2
kN.m/kg
Elongation
9
–
20
% strain
Compressive strength
130
–
160
MPa
Flexural modulus
78
–
82
GPa
Flexural strength (modulus of rupture)
130
–
160
MPa
Shear modulus
28.9
–
30.3
GPa
Bulk modulus
84.2
–
88.6
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
28
Hardness – Vickers
70
–
90
HV
Elastic stored energy (springs)
107
–
159
kJ/m3
Fatigue strength at 10^7 cycles
123
–
150
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
101
–
183
MPa
C90700 Impact & fracture properties
Fracture toughness
61.3
–
67.9
MPa.m0.5
Toughness (G)
47
–
57.7
kJ/m2
CuSn10 C90700 Cast Thermal properties
Melting point
887
–
1040
°C
Maximum service temperature
150
–
170
°C
Minimum service temperature
-273
°C
Thermal conductivity
58
–
63
W/m.°C
Specific heat capacity
376
–
392
J/kg.°C
Thermal expansion coefficient
18
–
19
µstrain/°C
Thermal shock resistance
87.4
–
109
°C
Thermal distortion resistance
3.11
–
3.43
MW/m
Latent heat of fusion
220
–
240
kJ/kg
C90700 Electrical properties
Electrical resistivity
14.8
–
16.6
µohm.cm
Electrical conductivity
10.4
–
11.6
%IACS
Galvanic potential
-0.24
–
-0.16
V
C90700 Magnetic properties
Magnetic type
Non-magnetic
C90700 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2980
–
3050
m/s
Mechanical loss coefficient (tan delta)
1.56e-4
–
2.37e-4
C90700 Processing properties
Metal casting
Excellent
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
36.6 m/min
Weldability Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Good
C90700 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuSn10 C90700 Cast Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible
C90700 Notes
CuSn10 C90700 Cast Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C90700 Standards with similar compositions
Czech Republic: CuSn10 to CSN 423119
Japan: CAC502A to JIS H5120
South Africa: Cu-Sn10 to SABS 200, Cu-Sn12P to SABS 200
USA: C90700, C90700 to ASTM B427, C90700 to ASTM B505, C90700 to CDA Datasheet, C90700 to SAE J462, C90800, C90800 to ASTM B30, C90800 to ASTM B427, UNS C90250, UNS C90700, UNS C90800