Home » Bronze Alloys » CuSn11P (C90710) Phosphor Bronze, Cast Material Data Sheet
CuSn11P (C90710) Phosphor Bronze, Cast Material Data Sheet
CuSn11P (C90710) Phosphor Bronze Material Data Sheet (Cast)
CuSn11P C90710 Cast Overview
CuSn11P C90710 cast is a cast bronze (UNS C90710), known as phosphor bronze. Condition: Cast. This CuSn11P C90710 cast material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C90710 bronze castings from Turkey (Türkiye)? Modulus Metal supplies C90710 bronze castings with in-house CNC machining and inspects them before shipment.
C90710 Designation
CuSn11P
UNS number
C90710
ISO name
CuSn11P
C90710 Typical uses
High-heat grade gears, bearings & bushes for heavy-duty and adequate lubrication, pump gears etc in corrosive conditions.
CuSn11P C90710 Cast Composition detail
Al (aluminum)
0
–
0.005
%
Cu (copper)
86
–
89.5
%
Fe (iron)
0
–
0.1
%
Ni (nickel)
0
–
0.1
%
P (phosphorus)
0.5
–
1.2
%
Pb (lead)
0
–
0.25
%
S (sulfur)
0
–
0.05
%
Sb (antimony)
0
–
0.2
%
Si (silicon)
0
–
0.005
%
Sn (tin)
10
–
12
%
Zn (zinc)
0
–
0.05
%
C90710 Physical properties
Density
8.8
–
8.82
g/cm3
CuSn11P C90710 Cast Mechanical properties
Young’s modulus
78
–
82
GPa
Specific stiffness
8.85
–
9.31
MN.m/kg
Yield strength (elastic limit)
170
–
230
MPa
Tensile strength
310
–
390
MPa
Specific strength
19.3
–
26.1
kN.m/kg
Elongation
2
–
8
% strain
Compressive strength
170
–
230
MPa
Flexural modulus
78
–
82
GPa
Flexural strength (modulus of rupture)
170
–
230
MPa
Shear modulus
28.9
–
30.3
GPa
Bulk modulus
84.2
–
88.6
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
25
Hardness – Vickers
95
–
150
HV
Elastic stored energy (springs)
184
–
324
kJ/m3
Fatigue strength at 10^7 cycles
150
–
174
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
128
–
203
MPa
C90710 Impact & fracture properties
Fracture toughness
50
–
59.4
MPa.m0.5
Toughness (G)
31.4
–
43.9
kJ/m2
CuSn11P C90710 Cast Thermal properties
Melting point
885
–
1040
°C
Maximum service temperature
150
–
170
°C
Minimum service temperature
-273
°C
Thermal conductivity
40
–
45
W/m.°C
Specific heat capacity
376
–
392
J/kg.°C
Thermal expansion coefficient
18
–
19
µstrain/°C
Thermal shock resistance
115
–
156
°C
Thermal distortion resistance
2.15
–
2.45
MW/m
Latent heat of fusion
220
–
240
kJ/kg
C90710 Electrical properties
Electrical resistivity
18.2
–
20.4
µohm.cm
Electrical conductivity
8.45
–
9.47
%IACS
Galvanic potential
-0.24
–
-0.16
V
C90710 Magnetic properties
Magnetic type
Non-magnetic
C90710 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2980
–
3050
m/s
Mechanical loss coefficient (tan delta)
7.6e-5
–
1.38e-4
C90710 Processing properties
Metal casting
Excellent
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
33.5 m/min
Weldability Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Excellent
C90710 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuSn11P C90710 Cast Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible
C90710 Notes
CuSn11P C90710 Cast Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C90710 Standards with similar compositions
Australia: C90710 to AS 2738, C90810 to AS 2738
Europe: CB481K to CEN EN 1982, CC481K to CEN EN 1982
International: CuSn10P to ISO 1338, CuSn10P to ISO 4382-1
USA: C90710, C90710 to CDA Datasheet, C90800, UNS C90710, UNS C90800, UNS C90810
Tradenames: ENDURANCE AA, HOLFOS B O, HOLFOS B O H T