Home » Bronze Alloys » C94100 Leaded Bronze 75-5-20, Cast Material Data Sheet
C94100 Leaded Bronze 75-5-20, Cast Material Data Sheet
C94100 Leaded Bronze 75-5-20 Material Data Sheet (Cast)
C94100 Cast Bronze Overview
C94100 cast bronze is a cast bronze (UNS C94100, EN CC497K), known as leaded bronze 75-5-20. Condition: Cast. This C94100 cast bronze material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C94100 bronze castings from Turkey (Türkiye)? Modulus Metal supplies C94100 bronze castings with in-house CNC machining and inspects them before shipment.
C94100 Designation
Copper Alloy: CuSn5Pb20 (UNS C94100)
UNS number
C94100
EN name
CC497K
ISO name
CuPb20Sn5
GB (Chinese) name
CuPb20Sn5
C94100 Typical uses
Steel-backed bearings for car and aero engines.
C94100 Cast Bronze Composition detail
Al (aluminum)
0
–
0.005
%
Cu (copper)
68.3
–
77.5
%
Fe (iron)
0
–
0.25
%
Ni (nickel)
0
–
1
%
P (phosphorus)
0
–
0.05
%
Pb (lead)
18
–
22
%
S (sulfur)
0
–
0.08
%
Sb (antimony)
0
–
0.8
%
Si (silicon)
0
–
0.005
%
Sn (tin)
4.5
–
6.5
%
Zn (zinc)
0
–
1
%
C94100 Physical properties
Density
8.95
–
9.05
g/cm3
C94100 Cast Bronze Mechanical properties
Young’s modulus
68
–
72
GPa
Specific stiffness
7.55
–
8
MN.m/kg
Yield strength (elastic limit)
60
–
100
MPa
Tensile strength
160
–
190
MPa
Specific strength
6.67
–
11.1
kN.m/kg
Elongation
5
–
10
% strain
Compressive strength
60
–
100
MPa
Flexural modulus
68
–
72
GPa
Flexural strength (modulus of rupture)
60
–
100
MPa
Shear modulus
25.2
–
26.6
GPa
Bulk modulus
73.4
–
77.8
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
30
Hardness – Vickers
45
–
65
HV
Elastic stored energy (springs)
27.1
–
67.9
kJ/m3
Fatigue strength at 10^7 cycles
97
–
109
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
86.3
–
123
MPa
C94100 Impact & fracture properties
Fracture toughness
76
–
90.5
MPa.m0.5
Toughness (G)
83
–
116
kJ/m2
C94100 Cast Bronze Thermal properties
Melting point
927
–
1060
°C
Maximum service temperature
180
–
190
°C
Minimum service temperature
-273
°C
Thermal conductivity
70
–
76
W/m.°C
Specific heat capacity
376
–
392
J/kg.°C
Thermal expansion coefficient
18
–
19
µstrain/°C
Thermal shock resistance
46.3
–
77.4
°C
Thermal distortion resistance
3.76
–
4.14
MW/m
Latent heat of fusion
220
–
240
kJ/kg
C94100 Electrical properties
Electrical resistivity
11.7
–
12.9
µohm.cm
Electrical conductivity
13.4
–
14.7
%IACS
Galvanic potential
-0.28
–
-0.2
V
C94100 Magnetic properties
Magnetic type
Non-magnetic
C94100 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2750
–
2830
m/s
Mechanical loss coefficient (tan delta)
4e-4
–
0.00111
C94100 Processing properties
Metal casting
Excellent
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
122 m/min
Weldability
Unsuitable
C94100 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Contains lead which lubricates, improving resistance.
Excellent
Flammability
Non-flammable
C94100 Cast Bronze Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible
C94100 Notes
C94100 Cast Bronze Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C94100 Standards with similar compositions
Australia: C94100 to AS 2738
USA: C94100, C94100 to ASTM B505, C94100 to ASTM B67, C94100 to CDA Datasheet, C94500, UNS C94100, UNS C94500