CuSn12 (C90810) Phosphor Bronze, Cast Material Data Sheet

CuSn12 (C90810) Phosphor Bronze Material Data Sheet (Cast)

CuSn12 C90810 Cast Overview

CuSn12 C90810 cast is a cast bronze (UNS C90810), known as phosphor bronze. Condition: Cast. This CuSn12 C90810 cast material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C90810 bronze castings from Turkey (Türkiye)? Modulus Metal supplies C90810 bronze castings with in-house CNC machining and inspects them before shipment.

C90810 Designation

CuSn12
UNS numberC90810
ISO nameCuSn10P

C90810 Typical uses

Gears & worm wheels (resistant to shock loads), heavily-loaded bearings.

CuSn12 C90810 Cast Composition detail

Al (aluminum)0–0.005%
Cu (copper)84.7–88.8%
Fe (iron)0–0.15%
Ni (nickel)0–0.5%
P (phosphorus)0.15–0.8%
Pb (lead)0–0.25%
S (sulfur)0–0.05%
Sb (antimony)0–0.2%
Si (silicon)0–0.005%
Sn (tin)11–13%
Zn (zinc)0–0.3%

C90810 Physical properties

Density8.8–8.82g/cm3

CuSn12 C90810 Cast Mechanical properties

Young’s modulus78–82GPa
Specific stiffness8.85–9.31MN.m/kg
Yield strength (elastic limit)170–200MPa
Tensile strength270–340MPa
Specific strength19.3–22.7kN.m/kg
Elongation3–7% strain
Compressive strength170–200MPa
Flexural modulus78–82GPa
Flexural strength (modulus of rupture)170–200MPa
Shear modulus28.9–30.3GPa
Bulk modulus84.2–88.6GPa
Poisson’s ratio0.34–0.35 
Shape factor26
Hardness – Vickers100–150HV
Elastic stored energy (springs)181–249kJ/m3
Fatigue strength at 10^7 cycles137–159MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
117–186MPa

C90810 Impact & fracture properties

Fracture toughness54.3–59.4MPa.m0.5
Toughness (G)36.8–44.2kJ/m2

CuSn12 C90810 Cast Thermal properties

Melting point867–1020°C
Maximum service temperature150–170°C
Minimum service temperature-273  °C
Thermal conductivity40–45W/m.°C
Specific heat capacity376–392J/kg.°C
Thermal expansion coefficient18–19µstrain/°C
Thermal shock resistance114–136°C
Thermal distortion resistance2.15–2.45MW/m
Latent heat of fusion220–240kJ/kg

C90810 Electrical properties

Electrical resistivity18.2–20.4µohm.cm
Electrical conductivity8.45–9.47%IACS
Galvanic potential-0.24–-0.16V

C90810 Magnetic properties

Magnetic typeNon-magnetic

C90810 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2980–3050m/s
Mechanical loss coefficient (tan delta)1e-4–1.38e-4 

C90810 Processing properties

Metal castingExcellent
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed33.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Excellent

C90810 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuSn12 C90810 Cast Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible

C90810 Notes

CuSn12 C90810 Cast Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C90810 Standards with similar compositions

Australia: 904D to AS 1565, C90810 to AS 2738
Japan: CAC502B to JIS H5120, CAC503B to JIS H5120, CAC503C to JIS H5121
USA: C90810, C90810 to CDA Datasheet, C90900, UNS C90810, UNS C90900