Home » Bronze Alloys » CuSn7Pb3 (C93100) Leaded Phosphor Bronze, Cast Material Data Sheet
CuSn7Pb3 (C93100) Leaded Phosphor Bronze, Cast Material Data Sheet
CuSn7Pb3 (C93100) Leaded Phosphor Bronze Material Data Sheet (Cast)
CuSn7Pb3 C93100 Cast Overview
CuSn7Pb3 C93100 cast is a cast bronze (UNS C93100), known as leaded phosphor bronze. Condition: Cast. This CuSn7Pb3 C93100 cast material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C93100 bronze castings from Turkey (Türkiye)? Modulus Metal supplies C93100 bronze castings with in-house CNC machining and inspects them before shipment.
C93100 Designation
CuSn7Pb3
UNS number
C93100
ISO name
CuSn8Pb4Zn1
C93100 Typical uses
Light-duty bearings and bushes.
CuSn7Pb3 C93100 Cast Composition detail
Al (aluminum)
0
–
0.005
%
Cu (copper)
81.4
–
91.5
%
Fe (iron)
0
–
0.25
%
Ni (nickel)
0
–
1
%
P (phosphorus)
0
–
1.5
%
Pb (lead)
2
–
5
%
S (sulfur)
0
–
0.05
%
Sb (antimony)
0
–
0.25
%
Si (silicon)
0
–
0.005
%
Sn (tin)
6.5
–
8.5
%
Zn (zinc)
0
–
2
%
C93100 Physical properties
Density
8.83
–
8.85
g/cm3
CuSn7Pb3 C93100 Cast Mechanical properties
Young’s modulus
74
–
76
GPa
Specific stiffness
8.37
–
8.6
MN.m/kg
Yield strength (elastic limit)
130
–
200
MPa
Tensile strength
270
–
360
MPa
Specific strength
14.7
–
22.6
kN.m/kg
Elongation
5
–
18
% strain
Compressive strength
130
–
200
MPa
Flexural modulus
74
–
76
GPa
Flexural strength (modulus of rupture)
130
–
200
MPa
Shear modulus
27.4
–
28.1
GPa
Bulk modulus
79.9
–
82.1
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
27
Hardness – Vickers
85
–
110
HV
Elastic stored energy (springs)
117
–
257
kJ/m3
Fatigue strength at 10^7 cycles
137
–
165
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
113
–
201
MPa
C93100 Impact & fracture properties
Fracture toughness
54.3
–
67.9
MPa.m0.5
Toughness (G)
39.7
–
60.8
kJ/m2
CuSn7Pb3 C93100 Cast Thermal properties
Melting point
882
–
1030
°C
Maximum service temperature
150
–
170
°C
Minimum service temperature
-273
°C
Thermal conductivity
58
–
63
W/m.°C
Specific heat capacity
376
–
392
J/kg.°C
Thermal expansion coefficient
18
–
19
µstrain/°C
Thermal shock resistance
93.6
–
144
°C
Thermal distortion resistance
3.11
–
3.43
MW/m
Latent heat of fusion
220
–
240
kJ/kg
C93100 Electrical properties
Electrical resistivity
14.8
–
16.6
µohm.cm
Electrical conductivity
10.4
–
11.6
%IACS
Galvanic potential
-0.24
–
-0.16
V
C93100 Magnetic properties
Magnetic type
Non-magnetic
C93100 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2890
–
2930
m/s
Mechanical loss coefficient (tan delta)
1e-4
–
2.37e-4
C93100 Processing properties
Metal casting
Excellent
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
61 m/min
Weldability
Unsuitable
C93100 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Contains lead which lubricates, improving resistance.
Excellent
Flammability
Non-flammable
CuSn7Pb3 C93100 Cast Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible
C93100 Notes
CuSn7Pb3 C93100 Cast Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.