Home » Bronze Alloys » CuSn8 (C52100) 9% Phosphor Bronze, Extra Hard Material Data Sheet
CuSn8 (C52100) 9% Phosphor Bronze, Extra Hard Material Data Sheet
CuSn8 (C52100) 9% Phosphor Bronze Material Data Sheet (Wrought, Extra Hard)
CuSn8 C52100 Extra Hard Overview
CuSn8 C52100 extra hard is a wrought bronze (UNS C52100, EN CW453K), known as 9% phosphor bronze. Condition: Extra hard. This CuSn8 C52100 extra hard material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C52100 bronze parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C52100 bronze parts in-house and inspects them before shipment.
C52100 Designation
CuSn8, wrought
Condition
Extra hard
UNS number
C52100
EN name
CW453K
ISO name
CuSn8
JIS (Japanese) name
C5210 / C5212
C52100 Typical uses
Heavy-duty springs and washers, pinions, gears, pump parts, bushings, clutch plates, bridge bearings, items for chemical & textile plant.
CuSn8 C52100 Extra Hard Composition detail
Cu (copper)
90.3
–
93
%
Fe (iron)
0
–
0.1
%
P (phosphorus)
0.03
–
0.35
%
Pb (lead)
0
–
0.05
%
Sn (tin)
7
–
9
%
Zn (zinc)
0
–
0.2
%
C52100 Physical properties
Density
8.5
–
8.52
g/cm3
CuSn8 C52100 Extra Hard Mechanical properties
Young’s modulus
105
–
110
GPa
Specific stiffness
12.3
–
12.9
MN.m/kg
Yield strength (elastic limit)
700
–
720
MPa
Tensile strength
830
–
870
MPa
Specific strength
82.3
–
84.6
kN.m/kg
Elongation
3.5
–
4
% strain
Compressive strength
700
–
720
MPa
Flexural modulus
105
–
110
GPa
Flexural strength (modulus of rupture)
700
–
720
MPa
Shear modulus
38.9
–
40.7
GPa
Bulk modulus
113
–
119
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
13
Hardness – Vickers
245
–
250
HV
Elastic stored energy (springs)
2260
–
2430
kJ/m3
Fatigue strength at 10^7 cycles
284
–
293
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
275
–
303
MPa
C52100 Impact & fracture properties
Fracture toughness
21.8
–
22.4
MPa.m0.5
Toughness (G)
4.39
–
4.71
kJ/m2
CuSn8 C52100 Extra Hard Thermal properties
Melting point
887
–
1040
°C
Maximum service temperature
160
–
170
°C
Minimum service temperature
-273
°C
Thermal conductivity
62
–
64
W/m.°C
Specific heat capacity
384
J/kg.°C
Thermal expansion coefficient
16.5
–
17.5
µstrain/°C
Thermal shock resistance
374
–
405
°C
Thermal distortion resistance
3.59
–
3.83
MW/m
Latent heat of fusion
220
–
240
kJ/kg
C52100 Electrical properties
Electrical resistivity
14.8
–
16.6
µohm.cm
Electrical conductivity
10.4
–
11.6
%IACS
Temperature dependence of resistivity
2
–
2.5
/°C
Galvanic potential
-0.23
–
-0.15
V
C52100 Magnetic properties
Magnetic type
Non-magnetic
C52100 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3510
–
3600
m/s
Mechanical loss coefficient (tan delta)
8e-6
C52100 Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Unsuitable
Metal press forming
Acceptable
Metal deep drawing
Limited use
Machining speed
30.5 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Excellent
C52100 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuSn8 C52100 Extra Hard Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible
C52100 Notes
CuSn8 C52100 Extra Hard Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C52100 Standards with similar compositions
Canada: HC.4.TJ80(521) to CSA
Czech Republic: CuSn8 to CSN 423015
Europe: CW453K to CEN EN 12163, CW453K to CEN EN 12166, CW453K to CEN EN 12167, CW453K to CEN EN 12449, CW453K to CEN EN 1652, CW453K to CEN EN 1654, CW459K to CEN EN 12163, CW459K to CEN EN 12449
Germany: 2.101 to DIN, CuSn8 to DIN
USA: C52100, C52100 to ASTM B103/B103M, C52100 to ASTM B139M, C52100 to ASTM B159M, C52100 to ASTM B888, ECuSn-C to AWS A5.6, MIL CuSn-C to MIL E-23765/3A, UNS C52100
Tradenames: 5210, ANACONDA (C) 521, BOLTON NO. 15 PHOSPHOR BRONZE, BRONZE DEVIL, C PHOSPHOR BRONZE, CARO, CUPRONAR 920C, ELEPHANT BRAND NO. 170 METAL, HARRIS PHOSPHOR BRONZE C, MILLER 200 PLUS GR. C, PHOSPHOR BRONZE, PHOSPHOR BRONZE (C) 353, PHOSPHOR BRONZE 8% C 521, PHOSPHOR BRONZE GRADE C, PHOSPHORBRONZE SN BZ 8, REVERE ALLOY NO. 521, RIVERSIDE PHOSPHOR BRONZE NO. 47, SEYMOUR 9230, SEYMOUR NO. 9225, SEYMOUR NO. 928, SUPER X PHOSPHOR BRONZE GR. C ALLOY 113, WATERBURY PBC, WIELAND FW8, ZINNBRONZE SNBZ8