Home » Bronze Alloys » C93700 Leaded Bronze 80-10-10, Cast Material Data Sheet
C93700 Leaded Bronze 80-10-10, Cast Material Data Sheet
C93700 Leaded Bronze 80-10-10 Material Data Sheet (Cast)
C93700 Cast Bronze Overview
C93700 cast bronze is a cast bronze (UNS C93700, EN CC495K), known as leaded bronze 80-10-10. Condition: Cast. This C93700 cast bronze material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C93700 bronze castings from Turkey (Türkiye)? Modulus Metal supplies C93700 bronze castings with in-house CNC machining and inspects them before shipment.
C93700 Designation
Copper Alloy: CuSn10Pb10 (UNS C93700)
UNS number
C93700
EN name
CC495K
ISO name
CuPb10Sn10
GB (Chinese) name
CuPb10Sn10
JIS (Japanese) name
LBC 3
C93700 Typical uses
Bearings and bushes to resist corrosion and poor lubrication (plasticity increases with lead content, making them suitable for minor misalignment and for use with soft steel shafts).
C93700 Cast Bronze Composition detail
Al (aluminum)
0
–
0.005
%
Cu (copper)
75.3
–
83
%
Fe (iron)
0
–
0.15
%
Ni (nickel)
0
–
1
%
P (phosphorus)
0
–
0.15
%
Pb (lead)
8
–
11
%
S (sulfur)
0
–
0.08
%
Sb (antimony)
0
–
0.5
%
Si (silicon)
0
–
0.005
%
Sn (tin)
9
–
11
%
Zn (zinc)
0
–
0.8
%
C93700 Physical properties
Density
8.85
–
8.87
g/cm3
C93700 Cast Bronze Mechanical properties
Young’s modulus
72
–
74
GPa
Specific stiffness
8.13
–
8.35
MN.m/kg
Yield strength (elastic limit)
80
–
130
MPa
Tensile strength
190
–
270
MPa
Specific strength
9.03
–
14.7
kN.m/kg
Elongation
5
–
15
% strain
Compressive strength
80
–
130
MPa
Flexural modulus
72
–
74
GPa
Flexural strength (modulus of rupture)
80
–
130
MPa
Shear modulus
26.6
–
27.4
GPa
Bulk modulus
77.8
–
79.9
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
29
Hardness – Vickers
65
–
85
HV
Elastic stored energy (springs)
46
–
110
kJ/m3
Fatigue strength at 10^7 cycles
109
–
137
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
86.8
–
172
MPa
C93700 Impact & fracture properties
Fracture toughness
67.9
–
82.6
MPa.m0.5
Toughness (G)
63.7
–
92.7
kJ/m2
C93700 Cast Bronze Thermal properties
Melting point
867
–
1020
°C
Maximum service temperature
180
–
190
°C
Minimum service temperature
-273
°C
Thermal conductivity
43
–
47
W/m.°C
Specific heat capacity
376
–
392
J/kg.°C
Thermal expansion coefficient
18
–
19
µstrain/°C
Thermal shock resistance
59.2
–
96.4
°C
Thermal distortion resistance
2.31
–
2.56
MW/m
Latent heat of fusion
220
–
240
kJ/kg
C93700 Electrical properties
Electrical resistivity
16.2
–
18.2
µohm.cm
Electrical conductivity
9.47
–
10.6
%IACS
Galvanic potential
-0.27
–
-0.19
V
C93700 Magnetic properties
Magnetic type
Non-magnetic
C93700 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2850
–
2890
m/s
Mechanical loss coefficient (tan delta)
2.37e-4
–
6.25e-4
C93700 Processing properties
Metal casting
Excellent
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
88.4 m/min
Weldability
Unsuitable
C93700 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Contains lead which lubricates, improving resistance.
Excellent
Flammability
Non-flammable
C93700 Cast Bronze Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible
C93700 Notes
C93700 Cast Bronze Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C93700 Standards with similar compositions
Australia: C93700 to AS 2738
Czech Republic: CuSn10Pb10 to CSN 423122
Europe: CB495K to CEN EN 1982
Germany: 2.1177 to DIN 17656, GB-CuPb10Sn to DIN 17656
Japan: CAC603 to JIS H5120, CAC603C to JIS H5121
Norway: 16540 to NS 16540
USA: C93700, C93700 to ASTM B22, C93700 to ASTM B271, C93700 to ASTM B30, C93700 to ASTM B584, C93700 to ASTM B66, C93700 to ASTM B763, C93700 to CDA Datasheet, C93700 to SAE J462, SAE 792 to SAE J460, UNS C93700