CuSn4 (C50900) 3% Phosphor Bronze, Half Hard Material Data Sheet

CuSn4 (C50900) 3% Phosphor Bronze Material Data Sheet (Wrought, Half Hard)

CuSn4 C50900 Half Hard Overview

CuSn4 C50900 half hard is a wrought bronze (UNS C50900, EN CW450K), known as 3% phosphor bronze. Condition: Half hard. This CuSn4 C50900 half hard material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C50900 bronze parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C50900 bronze parts in-house and inspects them before shipment.

C50900 Designation

CuSn4, wrought
ConditionHalf hard
UNS numberC50900
EN nameCW450K
ISO nameCuSn4
GB (Chinese) nameQSn4-0.3
JIS (Japanese) nameC5111

C50900 Typical uses

Tube plates for condensers & pressure vessels, bellows & diaphragms, masonry fixings, screws, bolts, rivets, washers, springs, clips, electrical contacts, switch parts, instrument components.

CuSn4 C50900 Half Hard Composition detail

Cu (copper)95.4–97.5%
Fe (iron)0–0.1%
P (phosphorus)0.03–0.3%
Pb (lead)0–0.05%
Sn (tin)2.5–3.8%
Zn (zinc)0–0.3%

C50900 Physical properties

Density8.83–8.85g/cm3

CuSn4 C50900 Half Hard Mechanical properties

Young’s modulus118–122GPa
Specific stiffness13.3–13.8MN.m/kg
Yield strength (elastic limit)390–400MPa
Tensile strength500–510MPa
Specific strength44.1–45.3kN.m/kg
Elongation12–15% strain
Compressive strength390–400MPa
Flexural modulus118–122GPa
Flexural strength (modulus of rupture)390–400MPa
Shear modulus43.7–45.1GPa
Bulk modulus127–132GPa
Poisson’s ratio0.34–0.35 
Shape factor22
Hardness – Vickers100–165HV
Hardness – Brinell88–143HB
Elastic stored energy (springs)631–670kJ/m3
Fatigue strength at 10^7 cycles204–207MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
200–211MPa

C50900 Impact & fracture properties

Fracture toughness34.5–35.2MPa.m0.5
Toughness (G)9.86–10.4kJ/m2

CuSn4 C50900 Half Hard Thermal properties

Melting point947–1070°C
Maximum service temperature150–160°C
Minimum service temperature-273  °C
Thermal conductivity84–86W/m.°C
Specific heat capacity385  J/kg.°C
Thermal expansion coefficient16.5–17.5µstrain/°C
Thermal shock resistance187–201°C
Thermal distortion resistance4.85–5.16MW/m
Latent heat of fusion220–240kJ/kg

C50900 Electrical properties

Electrical resistivity11.3–11.7µohm.cm
Electrical conductivity14.7–15.3%IACS
Temperature dependence of resistivity2–2.5/°C
Galvanic potential-0.21–-0.13V

C50900 Magnetic properties

Magnetic typeNon-magnetic

C50900 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3650–3720m/s
Mechanical loss coefficient (tan delta)2.5e-5–2.6e-5 

C50900 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingLimited use
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed33.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good

C50900 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuSn4 C50900 Half Hard Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible

C50900 Notes

CuSn4 C50900 Half Hard Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C50900 Standards with similar compositions

UK: PB101 to BS 2870, PB101 to BS 2875
USA: C50900, UNS C50800, UNS C50900
Tradenames: BOLTON NO. 12 PHOSPHOR BRONZE, BRONZE, PHOSPHOR GRADE A, ELEPHANT BRAND NO. 3 METAL, HI-10, M.S. BRONZE, PHOSPHOR BRONZE 301, RIVERSIDE GRADE E PHOSPHOR BRONZE, SEYMOUR 9370, SEYMOUR 971, SEYMOUR 9971, SUPER X PHOSPHOR BRONZE GR. E ALLOY 101