CuSn3Zn1 Coinage Bronze, Hard Material Data Sheet

CuSn3Zn1 Coinage Bronze Material Data Sheet (Wrought, Hard)

CuSn3Zn1 Hard Bronze Overview

CuSn3Zn1 hard bronze is a wrought bronze, known as coinage bronze. Condition: Hard. This CuSn3Zn1 hard bronze material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuSn3Zn1 bronze parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuSn3Zn1 bronze parts in-house and inspects them before shipment.

CuSn3Zn1 Designation

CuSn3Zn1, wrought
ConditionHard

CuSn3Zn1 Typical uses

Coins and medals.

CuSn3Zn1 Hard Bronze Composition detail

Cu (copper)95.5–97%
Sn (tin)2–3%
Zn (zinc)1–1.5%

CuSn3Zn1 Physical properties

Density8.84–8.85g/cm3

CuSn3Zn1 Hard Bronze Mechanical properties

Young’s modulus118–122GPa
Specific stiffness13.3–13.8MN.m/kg
Yield strength (elastic limit)350–450MPa
Tensile strength450–550MPa
Specific strength39.6–50.9kN.m/kg
Elongation8–10% strain
Compressive strength350–450MPa
Flexural modulus118–122GPa
Flexural strength (modulus of rupture)350–450MPa
Shear modulus43.7–45.1GPa
Bulk modulus127–132GPa
Poisson’s ratio0.34–0.35 
Shape factor22
Hardness – Vickers160–180HV
Elastic stored energy (springs)517–832kJ/m3
Fatigue strength at 10^7 cycles191–218MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
167–249MPa

CuSn3Zn1 Impact & fracture properties

Fracture toughness31.7–38MPa.m0.5
Toughness (G)8.43–12kJ/m2

CuSn3Zn1 Hard Bronze Thermal properties

Melting point947–1070°C
Maximum service temperature150–160°C
Minimum service temperature-273  °C
Thermal conductivity80–84W/m.°C
Specific heat capacity385  J/kg.°C
Thermal expansion coefficient16.5–17.5µstrain/°C
Thermal shock resistance171–222°C
Thermal distortion resistance4.64–5.01MW/m
Latent heat of fusion220–240kJ/kg

CuSn3Zn1 Electrical properties

Electrical resistivity6.92–11.5µohm.cm
Electrical conductivity15–24.9%IACS
Galvanic potential-0.21–-0.13V

CuSn3Zn1 Magnetic properties

Magnetic typeNon-magnetic

CuSn3Zn1 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3650–3710m/s
Mechanical loss coefficient (tan delta)2e-5–3.3e-5 

CuSn3Zn1 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed30.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good

CuSn3Zn1 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuSn3Zn1 Hard Bronze Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible

CuSn3Zn1 Notes

CuSn3Zn1 Hard Bronze Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuSn3Zn1 Standards with similar compositions

Tradenames: COINAGE BRONZE, DIAPHRAGM BRASS, ENGLISH PENNY BRONZE, MEDAL BRONZE-2, MUNZBRONZE, NBD NO. 20 A