CuSn8 (C52100) 9% Phosphor Bronze, Soft Material Data Sheet

CuSn8 (C52100) 9% Phosphor Bronze Material Data Sheet (Wrought, Soft)

CuSn8 C52100 Soft Overview

CuSn8 C52100 soft is a wrought bronze (UNS C52100, EN CW453K), known as 9% phosphor bronze. Condition: Soft. This CuSn8 C52100 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C52100 bronze parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C52100 bronze parts in-house and inspects them before shipment.

C52100 Designation

CuSn8, wrought
ConditionSoft
UNS numberC52100
EN nameCW453K
ISO nameCuSn8
JIS (Japanese) nameC5210 / C5212

C52100 Typical uses

Heavy-duty springs and washers, pinions, gears, pump parts, bushings, clutch plates, bridge bearings, items for chemical & textile plant.

CuSn8 C52100 Soft Composition detail

Cu (copper)90.3–93%
Fe (iron)0–0.1%
P (phosphorus)0.03–0.35%
Pb (lead)0–0.05%
Sn (tin)7–9%
Zn (zinc)0–0.2%

C52100 Physical properties

Density8.5–8.52g/cm3

CuSn8 C52100 Soft Mechanical properties

Young’s modulus105–110GPa
Specific stiffness12.3–12.9MN.m/kg
Yield strength (elastic limit)145–150MPa
Tensile strength410–420MPa
Specific strength17–17.6kN.m/kg
Elongation60–65% strain
Compressive strength145–150MPa
Flexural modulus105–110GPa
Flexural strength (modulus of rupture)145–150MPa
Shear modulus38.9–40.7GPa
Bulk modulus113–119GPa
Poisson’s ratio0.34–0.35 
Shape factor29
Hardness – Vickers85–90HV
Elastic stored energy (springs)97.2–105kJ/m3
Fatigue strength at 10^7 cycles180–183MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
176–188MPa

C52100 Impact & fracture properties

Fracture toughness63.3–64.4MPa.m0.5
Toughness (G)36.9–39kJ/m2

CuSn8 C52100 Soft Thermal properties

Melting point887–1040°C
Maximum service temperature160–170°C
Minimum service temperature-273  °C
Thermal conductivity62–64W/m.°C
Specific heat capacity384  J/kg.°C
Thermal expansion coefficient16.5–17.5µstrain/°C
Thermal shock resistance77.5–84.1°C
Thermal distortion resistance3.59–3.83MW/m
Latent heat of fusion220–240kJ/kg

C52100 Electrical properties

Electrical resistivity11.7–12.9µohm.cm
Electrical conductivity13.4–14.7%IACS
Temperature dependence of resistivity2–2.5/°C
Galvanic potential-0.23–-0.15V

C52100 Magnetic properties

Magnetic typeNon-magnetic

C52100 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3510–3600m/s
Mechanical loss coefficient (tan delta)1.78e-4–1.9e-4 

C52100 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingUnsuitable
Metal press formingExcellent
Metal deep drawingExcellent
Machining speed33.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Excellent

C52100 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuSn8 C52100 Soft Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible

C52100 Notes

CuSn8 C52100 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C52100 Standards with similar compositions

Canada: HC.4.TJ80(521) to CSA
Czech Republic: CuSn8 to CSN 423015
Europe: CW453K to CEN EN 12163, CW453K to CEN EN 12166, CW453K to CEN EN 12167, CW453K to CEN EN 12449, CW453K to CEN EN 1652, CW453K to CEN EN 1654, CW459K to CEN EN 12163, CW459K to CEN EN 12449
Germany: 2.101 to DIN, CuSn8 to DIN
USA: C52100, C52100 to ASTM B103/B103M, C52100 to ASTM B139M, C52100 to ASTM B159M, C52100 to ASTM B888, ECuSn-C to AWS A5.6, MIL CuSn-C to MIL E-23765/3A, UNS C52100
Tradenames: 5210, ANACONDA (C) 521, BOLTON NO. 15 PHOSPHOR BRONZE, BRONZE DEVIL, C PHOSPHOR BRONZE, CARO, CUPRONAR 920C, ELEPHANT BRAND NO. 170 METAL, HARRIS PHOSPHOR BRONZE C, MILLER 200 PLUS GR. C, PHOSPHOR BRONZE, PHOSPHOR BRONZE (C) 353, PHOSPHOR BRONZE 8% C 521, PHOSPHOR BRONZE GRADE C, PHOSPHORBRONZE SN BZ 8, REVERE ALLOY NO. 521, RIVERSIDE PHOSPHOR BRONZE NO. 47, SEYMOUR 9230, SEYMOUR NO. 9225, SEYMOUR NO. 928, SUPER X PHOSPHOR BRONZE GR. C ALLOY 113, WATERBURY PBC, WIELAND FW8, ZINNBRONZE SNBZ8