Resulfurized Free-Machining Steels Compared: AISI 1117, 1118, 12L14, 1137, 1141 and 1144 Composition, Properties and Machinability

Resulfurized steels, the AISI/SAE 11xx and 12xx series, are carbon steels with deliberately raised sulfur. The sulfur combines with manganese to form manganese sulfide inclusions that break chips and lubricate the cutting edge, so these grades machine much faster than plain carbon steels of similar strength. AISI 12L14 adds lead for even easier cutting. This post compares AISI 1117, 1118, 12L14, 1137, 1141 and 1144 for chemical composition, mechanical properties and machinability, with plain carbon AISI 1020 and AISI 1040 as reference. All values come from the linked material data sheets.

Resulfurized Steels Chemical Composition: AISI 1117, 1118, 12L14, 1137, 1141, 1144

GradeC (%)Mn (%)S (%)P (%)Pb (%)Si (%)
AISI 11170.14–0.21–1.30.08–0.130–0.04——
AISI 11180.14–0.21.3–1.60.08–0.130–0.04——
AISI 11370.32–0.391.35–1.650.08–0.130–0.04——
AISI 11410.37–0.451.35–1.650.08–0.130–0.04——
AISI 11440.4–0.481.35–1.650.24–0.330–0.04——
AISI 12L140–0.150.85–1.150.26–0.350.04–0.090.15–0.350–0.1
AISI 10200.17–0.230.3–0.60–0.050–0.04——
AISI 10400.37–0.440.6–0.90–0.050–0.04——

AISI 1117 and 1118 are low carbon case-hardening grades; 1137, 1141 and 1144 are medium carbon grades with higher manganese that can be through-hardened. AISI 12L14 has the highest sulfur and also contains lead. AISI 1020 and 1040 (reference rows) have the normal sulfur limit of 0.05% maximum.

Resulfurized Steels Mechanical Properties: As Rolled AISI 1117, 1118, 12L14, 1137, 1141, 1144

Grade and conditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
AISI 1117 As Rolled275–335435–540135–16526–40
AISI 1118 As Rolled285–350465–580143–17326–38
AISI 1137 As Rolled340–420560–695180–22022–34
AISI 1141 As Rolled320–395595–745180–22017–27
AISI 1144 As Rolled375–470630–775195–24016–26
AISI 12L14 As Rolled342–517380–570115–25010–17
AISI 1020 As Rolled295–365395–500135–16528–43
AISI 1040 As Rolled375–460565–690188–22820–30

Resulfurized Steels Mechanical Properties: Annealed and Normalized

Grade and conditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
AISI 1117 Annealed250–310385–475118–14026–40
AISI 1117 Normalized270–335415–520130–16026–40
AISI 1118 Annealed255–315405–495128–15027–42
AISI 1118 Normalized285–355425–530135–16526–40
AISI 1137 Annealed305–380520–645160–20021–33
AISI 1137 Normalized355–435595–740185–22518–27
AISI 1141 Annealed315–390540–660150–19020–31
AISI 1141 Normalized365–445645–780188–22818–28
AISI 1144 Annealed310–385525–645155–19020–30
AISI 1144 Normalized360–440600–740180–22516–26
AISI 1020 Annealed265–325355–435110–13028–43
AISI 1020 Normalized310–350395–490125–15028–43
AISI 1040 Annealed315–390475–575143–17324–36
AISI 1040 Normalized335–415530–650160–19522–34

Resulfurized Steels Machinability: Machining Speed of AISI 1117, 1118, 12L14, 1137, 1141, 1144

GradeAnnealed (m/min)As rolled (m/min)Normalized (m/min)
AISI 111745.742.745.7
AISI 111845.742.745.7
AISI 113736.633.530.5
AISI 114136.630.529.9
AISI 114445.736.636.6
AISI 12L14—45.7—
AISI 1020 (reference)45.736.639.6
AISI 1040 (reference)33.525.629.3
Machining speed, as rolled (m/min)AISI 111742.7AISI 111842.7AISI 113733.5AISI 114130.5AISI 114436.6AISI 12L1445.7AISI 1020 (ref.)36.6AISI 1040 (ref.)25.6

In the as rolled condition the highest machining speed in these data sheets belongs to AISI 12L14 (45.7 m/min). At a similar carbon level the resulfurized grades cut faster than their plain carbon counterparts: AISI 1117, 1118 and 12L14 are faster than plain AISI 1020, and AISI 1137, 1141 and 1144 are faster than plain AISI 1040. The trade-off is lower transverse ductility and poorer weldability, because the sulfide inclusions are elongated in the rolling direction; resulfurized grades are therefore not recommended for welded or heavily cold-formed parts.

Resulfurized Steels Strength Charts: As Rolled

Tensile strength, as rolled (MPa)AISI 1117435–540AISI 1118465–580AISI 1137560–695AISI 1141595–745AISI 1144630–775AISI 12L14380–570AISI 1020 (ref.)395–500AISI 1040 (ref.)565–690
Hardness, as rolled (HV)AISI 1117135–165AISI 1118143–173AISI 1137180–220AISI 1141180–220AISI 1144195–240AISI 12L14115–250AISI 1020 (ref.)135–165AISI 1040 (ref.)188–228

Choosing Between Resulfurized Steels

Choose AISI 12L14 when machining speed and surface finish matter most and the part is lightly stressed. AISI 1117 and 1118 suit carburized or case-hardened parts that need a hard surface over a tough core. AISI 1137, 1141 and 1144 give higher strength in the as rolled or quenched and tempered condition for shafts, studs and spindles, while still machining easily. AISI 1117 | AISI 1118 | AISI 1137 | AISI 1141 | AISI 1144 | AISI 12L14

Looking for free-machining steel parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1117, 1144 and 12L14 parts in-house on automatic and CNC lathes, and inspects them before shipment.