AISI 1118 normalized is AISI 1118 resulfurized low carbon steel (UNS G11180) in the normalized condition. This AISI 1118 normalized material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1118 conditions in our AISI 1118 yield, tensile and hardness comparison. See also the resulfurized free-machining steels comparison. Looking for AISI 1118 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1118 steel parts in-house and inspects them before shipment.
AISI 1118 Normalized Designation
AISI 1118
Condition
Normalized
UNS number
G11180
US name
ASTM G11180, ASTM 11L18, ASTM 1118, ~ASTM D
AISI 1118 Normalized Typical uses
General construction, general mechanical engineering, automotive, tools, axles, gears, springs.
AISI 1118 Normalized Composition detail
C (carbon)
0.14
–
0.2
%
Fe (iron)
98
–
98.5
%
Mn (manganese)
1.3
–
1.6
%
P (phosphorus)
0
–
0.04
%
S (sulfur)
0.08
–
0.13
%
AISI 1118 Normalized Physical properties
Density
7.8
–
7.9
g/cm3
AISI 1118 Normalized Mechanical properties
Young’s modulus
205
–
215
GPa
Specific stiffness
26.1
–
27.4
MN.m/kg
Yield strength (elastic limit)
285
–
355
MPa
Tensile strength
425
–
530
MPa
Specific strength
36.3
–
45.2
kN.m/kg
Elongation
26
–
40
% strain
Compressive strength
285
–
355
MPa
Flexural modulus
205
–
215
GPa
Flexural strength (modulus of rupture)
285
–
355
MPa
Shear modulus
79
–
84
GPa
Bulk modulus
158
–
175
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
60
Hardness – Vickers
135
–
165
HV
Elastic stored energy (springs)
195
–
297
kJ/m3
Fatigue strength at 10^7 cycles
235
–
275
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
202
–
320
MPa
AISI 1118 Normalized Impact & fracture properties
Fracture toughness
46
–
75
MPa.m0.5
Toughness (G)
10.6
–
25.5
kJ/m2
AISI 1118 Normalized Thermal properties
Melting point
1490
–
1530
°C
Maximum service temperature
343
–
357
°C
Minimum service temperature
-63
–
-38
°C
Thermal conductivity
49
–
54
W/m.°C
Specific heat capacity
460
–
500
J/kg.°C
Thermal expansion coefficient
11.5
–
13
µstrain/°C
Thermal shock resistance
109
–
141
°C
Thermal distortion resistance
3.89
–
4.55
MW/m
Latent heat of fusion
270
–
275
kJ/kg
AISI 1118 Normalized Electrical properties
Electrical resistivity
15
–
20
µohm.cm
Electrical conductivity
8.62
–
11.5
%IACS
Galvanic potential
-0.52
–
-0.44
V
AISI 1118 Normalized Magnetic properties
Magnetic type
Magnetic
AISI 1118 Normalized Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5110
–
5240
m/s
Mechanical loss coefficient (tan delta)
9.6e-4
–
0.00121
AISI 1118 Normalized Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Excellent
Metal press forming
Acceptable
Metal deep drawing
Limited use
Machining speed
45.7 m/min
Weldability Notes: Preheating and post weld heat treatments may be required
Good
Carbon equivalency
0.357 – 0.467
AISI 1118 Normalized Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
Flammability
Non-flammable
AISI 1118 Normalized Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Not susceptible
AISI 1118 Normalized Standards with similar compositions
Argentina: IRAM 1118 to IAS
Canada: C1118 to CSA 95-1/1
India: 20Mn2 to IS 6967
Mexico: 1118 to NMX-B-301
Pan America: 1024 to COPANT 333, 1118 to COPANT 330, 1118 to COPANT 331, 1118 to COPANT 514
UK: 174H20 to BS 970/1, 175H23 to BS 970/1
USA: 1118, 1118 to ASTM A29/A29M, 1118 to ASTM A519, 1118 to FED QQ-S-00643, 1118 to FED QQ-S-633A, 1118 to SAE J403, 11L18 to ASTM A519, C1118 to FED QQ-S-637A, G11180 to ASTM A510/A510M, G11180 to ASTM A576-90b, MIL-S-16124 to MIL-S-16124, MIL-S-16611 to MIL-S-16611, UNS G11180