How do the AISI 1095 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength, hardness, elongation and machining speed of AISI 1095 high carbon steel (UNS G10950) side by side for 13 conditions: annealed, as rolled, normalized, oil quenched & tempered at 205°C, oil quenched & tempered at 315°C, oil quenched & tempered at 425°C, oil quenched & tempered at 540°C, oil quenched & tempered at 650°C, water quenched & tempered at 205°C, water quenched & tempered at 315°C, water quenched & tempered at 425°C, water quenched & tempered at 540°C, water quenched & tempered at 650°C. All values are taken from the individual AISI 1095 material data sheets linked below.
AISI 1095 Yield, Tensile and Hardness by Condition
| Condition | Yield strength (MPa) | Tensile strength (MPa) | Hardness (HV) | Elongation (%) | Machining speed (m/min) |
|---|---|---|---|---|---|
| Annealed | 340–420 | 590–720 | 180–220 | 10–16 | 24.1 |
| As Rolled | 510–635 | 865–1070 | 270–330 | 7–11 | 15.8 |
| Normalized | 450–550 | 910–1120 | 270–330 | 7.5–11.5 | 15.5 |
| Oil Quenched & Tempered at 205°C | 740–915 | 1160–1420 | 370–430 | 8–12 | 11.6 |
| Oil Quenched & Tempered at 315°C | 730–895 | 1130–1400 | 350–410 | 8–12 | 11.9 |
| Oil Quenched & Tempered at 425°C | 690–855 | 1090–1340 | 335–395 | 9.5–14.5 | 12.5 |
| Oil Quenched & Tempered at 540°C | 605–750 | 980–1200 | 300–350 | 12–18 | 14.3 |
| Oil Quenched & Tempered at 650°C | 495–610 | 805–990 | 250–300 | 17–25 | 17.1 |
| Water Quenched & Tempered at 205°C | 940–1160 | 1340–1640 | 550–650 | 8–12 | 8.23 |
| Water Quenched & Tempered at 315°C | 925–1140 | 1310–1620 | 490–580 | 9–13 | 8.84 |
| Water Quenched & Tempered at 425°C | 855–1060 | 1230–1520 | 360–430 | 10.5–15.5 | 11.3 |
| Water Quenched & Tempered at 540°C | 680–840 | 1030–1260 | 265–325 | 12–18 | 14.9 |
| Water Quenched & Tempered at 650°C | 525–650 | 755–930 | 220–260 | 16–24 | 19.2 |
AISI 1095 Differences Compared with Annealed
The table below shows how much each AISI 1095 condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength, hardness or elongation.
| Condition | Yield strength | Tensile strength | Hardness | Elongation |
|---|---|---|---|---|
| As Rolled | +51% | +48% | +50% | -31% |
| Normalized | +32% | +55% | +50% | -27% |
| Oil Quenched & Tempered at 205°C | +118% | +97% | +100% | -23% |
| Oil Quenched & Tempered at 315°C | +114% | +93% | +90% | -23% |
| Oil Quenched & Tempered at 425°C | +103% | +85% | +82% | -8% |
| Oil Quenched & Tempered at 540°C | +78% | +66% | +62% | +15% |
| Oil Quenched & Tempered at 650°C | +45% | +37% | +38% | +62% |
| Water Quenched & Tempered at 205°C | +176% | +127% | +200% | -23% |
| Water Quenched & Tempered at 315°C | +172% | +124% | +168% | -15% |
| Water Quenched & Tempered at 425°C | +152% | +110% | +98% | +0% |
| Water Quenched & Tempered at 540°C | +100% | +75% | +48% | +15% |
| Water Quenched & Tempered at 650°C | +55% | +29% | +20% | +54% |
AISI 1095 Oil Quenched vs Water Quenched
Water removes heat faster than oil, so water quenched AISI 1095 forms more martensite and comes out harder and stronger, but with a higher risk of distortion and quench cracking. The table compares AISI 1095 oil quenched and water quenched material tempered at the same temperature, and shows the difference of water quenching relative to oil quenching (mid-points).
| Tempered at | Yield oil / water (MPa) | Yield diff. | Tensile oil / water (MPa) | Tensile diff. | Hardness oil / water (HV) | Hardness diff. |
|---|---|---|---|---|---|---|
| 205°C | 740–915 / 940–1160 | +27% | 1160–1420 / 1340–1640 | +16% | 370–430 / 550–650 | +50% |
| 315°C | 730–895 / 925–1140 | +27% | 1130–1400 / 1310–1620 | +16% | 350–410 / 490–580 | +41% |
| 425°C | 690–855 / 855–1060 | +24% | 1090–1340 / 1230–1520 | +13% | 335–395 / 360–430 | +8% |
| 540°C | 605–750 / 680–840 | +12% | 980–1200 / 1030–1260 | +5% | 300–350 / 265–325 | -9% |
| 650°C | 495–610 / 525–650 | +6% | 805–990 / 755–930 | -6% | 250–300 / 220–260 | -13% |
AISI 1095 Strength and Hardness Charts
Oil quenched & tempered Water quenched & tempered. Dark bar = minimum, light bar = maximum of the range.
AISI 1095 Heat Treatment Key Points
The highest tensile strength of AISI 1095 in these data sheets is reached in the water quenched & tempered at 205°C condition (1340–1640 MPa). The softest condition is annealed (180–220 HV), with a machining speed of 24.1 m/min, which is usually preferred for machining and forming. For oil quenched AISI 1095, raising the tempering temperature from 205°C to 650°C lowers hardness from 370–430 HV to 250–300 HV, trading strength for toughness and ductility. For water quenched AISI 1095, raising the tempering temperature from 205°C to 650°C lowers hardness from 550–650 HV to 220–260 HV, trading strength for toughness and ductility.
AISI 1095 Material Data Sheets
AISI 1095 Annealed | AISI 1095 As Rolled | AISI 1095 Normalized | AISI 1095 Oil Quenched & Tempered at 205°C | AISI 1095 Oil Quenched & Tempered at 315°C | AISI 1095 Oil Quenched & Tempered at 425°C | AISI 1095 Oil Quenched & Tempered at 540°C | AISI 1095 Oil Quenched & Tempered at 650°C | AISI 1095 Water Quenched & Tempered at 205°C | AISI 1095 Water Quenched & Tempered at 315°C | AISI 1095 Water Quenched & Tempered at 425°C | AISI 1095 Water Quenched & Tempered at 540°C | AISI 1095 Water Quenched & Tempered at 650°C | All AISI 1095 conditions