AISI 1080 Annealed vs As Rolled vs Normalized vs Oil Quenched & Tempered (205–650°C): Yield, Tensile & Hardness Compared

How do the AISI 1080 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength, hardness, elongation and machining speed of AISI 1080 high carbon steel (UNS G10800) side by side for 8 conditions: annealed, as rolled, normalized, oil quenched & tempered at 205°C, oil quenched & tempered at 315°C, oil quenched & tempered at 425°C, oil quenched & tempered at 540°C, oil quenched & tempered at 650°C. All values are taken from the individual AISI 1080 material data sheets linked below.

AISI 1080 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)Machining speed (m/min)
Annealed335–415550–680160–20020–3027.7
As Rolled525–650865–975270–33010–1416.8
Normalized470–580905–1120270–3309–1316.2
Oil Quenched & Tempered at 205°C880–10801180–1450360–42010–1412.2
Oil Quenched & Tempered at 315°C880–10801170–1440360–42010–1412.2
Oil Quenched & Tempered at 425°C855–10501160–1430350–41011–1512.5
Oil Quenched & Tempered at 540°C725–8901020–1250300–35013–1914.6
Oil Quenched & Tempered at 650°C540–660800–980240–28017–2518.6

AISI 1080 Differences Compared with Annealed

The table below shows how much each AISI 1080 condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength, hardness or elongation.

ConditionYield strengthTensile strengthHardnessElongation
As Rolled+57%+50%+67%-52%
Normalized+40%+65%+67%-56%
Oil Quenched & Tempered at 205°C+161%+114%+117%-52%
Oil Quenched & Tempered at 315°C+161%+112%+117%-52%
Oil Quenched & Tempered at 425°C+154%+111%+111%-48%
Oil Quenched & Tempered at 540°C+115%+85%+81%-36%
Oil Quenched & Tempered at 650°C+60%+45%+44%-16%

AISI 1080 Strength and Hardness Charts

AISI 1080 Yield strength by condition (MPa)Annealed335–415As Rolled525–650Normalized470–580OQ&T 205°C880–1080OQ&T 315°C880–1080OQ&T 425°C855–1050OQ&T 540°C725–890OQ&T 650°C540–660
AISI 1080 Tensile strength by condition (MPa)Annealed550–680As Rolled865–975Normalized905–1120OQ&T 205°C1180–1450OQ&T 315°C1170–1440OQ&T 425°C1160–1430OQ&T 540°C1020–1250OQ&T 650°C800–980
AISI 1080 Hardness by condition (HV)Annealed160–200As Rolled270–330Normalized270–330OQ&T 205°C360–420OQ&T 315°C360–420OQ&T 425°C350–410OQ&T 540°C300–350OQ&T 650°C240–280

AISI 1080 Heat Treatment Key Points

The highest tensile strength of AISI 1080 in these data sheets is reached in the oil quenched & tempered at 205°C condition (1180–1450 MPa). The softest condition is annealed (160–200 HV), with a machining speed of 27.7 m/min, which is usually preferred for machining and forming. For oil quenched AISI 1080, raising the tempering temperature from 205°C to 650°C lowers hardness from 360–420 HV to 240–280 HV, trading strength for toughness and ductility.

AISI 1080 Material Data Sheets

AISI 1080 Annealed | AISI 1080 As Rolled | AISI 1080 Normalized | AISI 1080 Oil Quenched & Tempered at 205°C | AISI 1080 Oil Quenched & Tempered at 315°C | AISI 1080 Oil Quenched & Tempered at 425°C | AISI 1080 Oil Quenched & Tempered at 540°C | AISI 1080 Oil Quenched & Tempered at 650°C | All AISI 1080 conditions