AISI 12L14 as rolled is AISI 12L14 leaded resulfurized low carbon steel (UNS G12144, EN 11SMnPb37) in the as rolled condition. This AISI 12L14 as rolled material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. See also the resulfurized free-machining steels comparison. Looking for AISI 12L14 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 12L14 steel parts in-house and inspects them before shipment.
11SMnPb37, 11SMnPb30, 9SMnPb28 to BS EN 10087, BS EN 10277; S300Pb to NF A35 561
EN number
1.0737, 1.0718, 1.9718
JIS (Japanese) name
SUM24L to JIS G4804
Tradenames
LEDLOY 1214, Usaled, AMER-LED
AISI 12L14 As Rolled Typical uses
Free-machining / free-cutting steel for automatic screw machine and tool products, shafts, bolts, fasteners, cams, lightly stressed fasteners, for the automotive and general engineering industries.
AISI 12L14 As Rolled Composition detail
C (carbon)
0
–
0.15
%
Fe (iron)
97.8
–
98.7
%
Mn (manganese)
0.85
–
1.15
%
P (phosphorus)
0.04
–
0.09
%
Pb (lead)
0.15
–
0.35
%
S (sulfur)
0.26
–
0.35
%
Si (silicon)
0
–
0.1
%
AISI 12L14 As Rolled Physical properties
Density
7.83
–
7.91
g/cm3
AISI 12L14 As Rolled Mechanical properties
Young’s modulus
196
–
204
GPa
Specific stiffness
24.9
–
25.9
MN.m/kg
Yield strength (elastic limit)
342
–
517
MPa
Tensile strength
380
–
570
MPa
Specific strength
43.5
–
65.7
kN.m/kg
Elongation
10
–
17
% strain
Compressive strength
342
–
517
MPa
Flexural modulus
196
–
204
GPa
Flexural strength (modulus of rupture)
276
–
322
MPa
Shear modulus
77.7
–
82.4
GPa
Bulk modulus
152
–
168
GPa
Poisson’s ratio
0.29
Shape factor
52
Hardness – Vickers
115
–
250
HV
Hardness – Rockwell B
68
–
84
HRB
Hardness – Brinell
121
–
174
HB
Elastic stored energy (springs)
303
–
645
kJ/m3
Fatigue strength at 10^7 cycles
171
–
199
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
126
–
269
MPa
AISI 12L14 As Rolled Impact & fracture properties
Fracture toughness
76
–
92
MPa.m0.5
Toughness (G)
29.1
–
42
kJ/m2
AISI 12L14 As Rolled Thermal properties
Melting point
1490
–
1530
°C
Maximum service temperature
343
–
357
°C
Minimum service temperature
-63
–
-38
°C
Thermal conductivity
52
–
55
W/m.°C
Specific heat capacity
460
–
472
J/kg.°C
Thermal expansion coefficient
11.5
µstrain/°C
Thermal shock resistance
149
–
225
°C
Thermal distortion resistance
4.52
–
4.78
MW/m
Latent heat of fusion
270
–
275
kJ/kg
AISI 12L14 As Rolled Electrical properties
Electrical resistivity
12
–
17.4
µohm.cm
Electrical conductivity
9.91
–
14.4
%IACS
Galvanic potential
-0.52
–
-0.44
V
AISI 12L14 As Rolled Magnetic properties
Magnetic type
Magnetic
AISI 12L14 As Rolled Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
4990
–
5090
m/s
AISI 12L14 As Rolled Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Excellent
Metal press forming
Acceptable
Metal deep drawing
Unsuitable
Machining speed
45.7 m/min
Weldability Notes: Preheating and post weld heat treatments may be required, and contains hazardous elements
Poor
Weldability – TIG
Not recommended
Carbon equivalency
0.028 – 0.192
AISI 12L14 As Rolled Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
Flammability
Non-flammable
AISI 12L14 As Rolled Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia