AISI 1117 as rolled is AISI 1117 resulfurized low carbon steel (UNS G11170) in the as rolled condition. This AISI 1117 as rolled material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1117 conditions in our AISI 1117 yield, tensile and hardness comparison. See also the resulfurized free-machining steels comparison. Looking for AISI 1117 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1117 steel parts in-house and inspects them before shipment.
AISI 1117 As Rolled Designation
AISI 1117
Condition
As rolled
UNS number
G11170
US name
ASTM G11170, ASTM 1117 Class A, ASTM 1117, AMS 5022
GB (Chinese) name
~Y20
JIS (Japanese) name
SUM31L, SUM31
AISI 1117 As Rolled Typical uses
Lightly stressed parts, e.g. camshafts, selector forks, ratchets, tappets
AISI 1117 As Rolled Composition detail
C (carbon)
0.14
–
0.2
%
Fe (iron)
98.3
–
98.8
%
Mn (manganese)
1
–
1.3
%
P (phosphorus)
0
–
0.04
%
S (sulfur)
0.08
–
0.13
%
AISI 1117 As Rolled Physical properties
Density
7.8
–
7.9
g/cm3
AISI 1117 As Rolled Mechanical properties
Young’s modulus
205
–
215
GPa
Specific stiffness
26.1
–
27.4
MN.m/kg
Yield strength (elastic limit)
275
–
335
MPa
Tensile strength
435
–
540
MPa
Specific strength
35
–
42.7
kN.m/kg
Elongation
26
–
40
% strain
Compressive strength
275
–
335
MPa
Flexural modulus
205
–
215
GPa
Flexural strength (modulus of rupture)
275
–
335
MPa
Shear modulus
79
–
84
GPa
Bulk modulus
158
–
175
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
61
Hardness – Vickers
135
–
165
HV
Elastic stored energy (springs)
182
–
265
kJ/m3
Fatigue strength at 10^7 cycles
239
–
279
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
206
–
324
MPa
AISI 1117 As Rolled Impact & fracture properties
Fracture toughness
50
–
79
MPa.m0.5
Toughness (G)
12.4
–
28.5
kJ/m2
AISI 1117 As Rolled Thermal properties
Melting point
1490
–
1530
°C
Maximum service temperature
343
–
357
°C
Minimum service temperature
-63
–
-38
°C
Thermal conductivity
50
–
54
W/m.°C
Specific heat capacity
460
–
500
J/kg.°C
Thermal expansion coefficient
11.5
–
13
µstrain/°C
Thermal shock resistance
105
–
133
°C
Thermal distortion resistance
3.96
–
4.57
MW/m
Latent heat of fusion
270
–
275
kJ/kg
AISI 1117 As Rolled Electrical properties
Electrical resistivity
15
–
20
µohm.cm
Electrical conductivity
8.62
–
11.5
%IACS
Galvanic potential
-0.52
–
-0.44
V
AISI 1117 As Rolled Magnetic properties
Magnetic type
Magnetic
AISI 1117 As Rolled Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5110
–
5240
m/s
Mechanical loss coefficient (tan delta)
9.8e-4
–
0.00122
AISI 1117 As Rolled Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Excellent
Metal press forming
Acceptable
Metal deep drawing
Limited use
Machining speed
42.7 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Poor
Carbon equivalency
0.307 – 0.417
AISI 1117 As Rolled Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
Flammability
Non-flammable
AISI 1117 As Rolled Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Not susceptible
AISI 1117 As Rolled Notes
AISI 1117 As Rolled Warning
Free cutting’ steel – in common with all such steels, it is not recommended where welding is involved.
AISI 1117 As Rolled Other notes
Designed for oil hardening, but can be water quenched for maximum case hardness.
AISI 1117 As Rolled Standards with similar compositions
Canada: C1117 to CSA 94-1/1, CL.1.C1117 to CSA STAN95-1-1
India: A-N to IS 3945, B-N to IS 3945
Italy: CF17SMnPb10 to UNI 4838
Japan: SUM31 to JIS G4804, SUM31L to JIS G4804
Mexico: 1116 to NMX-B-301, 1117 to NMX-B-301
Pan America: 1117 to COPANT 330, 1117 to COPANT 331, 1117 to COPANT 333
UK: 15SMn13 to BS EN 10277-3, 170H15 to BS 970/1, 173H15 to BS 970/1, 173H16 to BS 970/1, 210A15 to BS 970/1, 210M15 to BS 970/1, 220M07 to BS 970/1
USA: 1114, 1116, 1116 to ASTM A29/A29M, 1117, 1117 Class A to ASTM A311/A311M, 1117 to ASTM A29/A29M, 1117 to ASTM A512-96, 1117 to MIL-S-18411, 1117 to SAE J403, 1120, 5022 to AMS 5022L, G11160 to ASTM A510/A510M, G11160 to ASTM A576-90b, G11170 to ASTM A510/A510M, G11170 to ASTM A576-90b, UNS G11160, UNS G11170, UNS K11711