Resulfurized steels, the AISI/SAE 11xx and 12xx series, are carbon steels with deliberately raised sulfur. The sulfur combines with manganese to form manganese sulfide inclusions that break chips and lubricate the cutting edge, so these grades machine much faster than plain carbon steels of similar strength. AISI 12L14 adds lead for even easier cutting. This post compares AISI 1117, 1118, 12L14, 1137, 1141 and 1144 for chemical composition, mechanical properties and machinability, with plain carbon AISI 1020 and AISI 1040 as reference. All values come from the linked material data sheets.
Resulfurized Steels Chemical Composition: AISI 1117, 1118, 12L14, 1137, 1141, 1144
| Grade | C (%) | Mn (%) | S (%) | P (%) | Pb (%) | Si (%) |
|---|---|---|---|---|---|---|
| AISI 1117 | 0.14–0.2 | 1–1.3 | 0.08–0.13 | 0–0.04 | — | — |
| AISI 1118 | 0.14–0.2 | 1.3–1.6 | 0.08–0.13 | 0–0.04 | — | — |
| AISI 1137 | 0.32–0.39 | 1.35–1.65 | 0.08–0.13 | 0–0.04 | — | — |
| AISI 1141 | 0.37–0.45 | 1.35–1.65 | 0.08–0.13 | 0–0.04 | — | — |
| AISI 1144 | 0.4–0.48 | 1.35–1.65 | 0.24–0.33 | 0–0.04 | — | — |
| AISI 12L14 | 0–0.15 | 0.85–1.15 | 0.26–0.35 | 0.04–0.09 | 0.15–0.35 | 0–0.1 |
| AISI 1020 | 0.17–0.23 | 0.3–0.6 | 0–0.05 | 0–0.04 | — | — |
| AISI 1040 | 0.37–0.44 | 0.6–0.9 | 0–0.05 | 0–0.04 | — | — |
AISI 1117 and 1118 are low carbon case-hardening grades; 1137, 1141 and 1144 are medium carbon grades with higher manganese that can be through-hardened. AISI 12L14 has the highest sulfur and also contains lead. AISI 1020 and 1040 (reference rows) have the normal sulfur limit of 0.05% maximum.
Resulfurized Steels Mechanical Properties: As Rolled AISI 1117, 1118, 12L14, 1137, 1141, 1144
| Grade and condition | Yield strength (MPa) | Tensile strength (MPa) | Hardness (HV) | Elongation (%) |
|---|---|---|---|---|
| AISI 1117 As Rolled | 275–335 | 435–540 | 135–165 | 26–40 |
| AISI 1118 As Rolled | 285–350 | 465–580 | 143–173 | 26–38 |
| AISI 1137 As Rolled | 340–420 | 560–695 | 180–220 | 22–34 |
| AISI 1141 As Rolled | 320–395 | 595–745 | 180–220 | 17–27 |
| AISI 1144 As Rolled | 375–470 | 630–775 | 195–240 | 16–26 |
| AISI 12L14 As Rolled | 342–517 | 380–570 | 115–250 | 10–17 |
| AISI 1020 As Rolled | 295–365 | 395–500 | 135–165 | 28–43 |
| AISI 1040 As Rolled | 375–460 | 565–690 | 188–228 | 20–30 |
Resulfurized Steels Mechanical Properties: Annealed and Normalized
| Grade and condition | Yield strength (MPa) | Tensile strength (MPa) | Hardness (HV) | Elongation (%) |
|---|---|---|---|---|
| AISI 1117 Annealed | 250–310 | 385–475 | 118–140 | 26–40 |
| AISI 1117 Normalized | 270–335 | 415–520 | 130–160 | 26–40 |
| AISI 1118 Annealed | 255–315 | 405–495 | 128–150 | 27–42 |
| AISI 1118 Normalized | 285–355 | 425–530 | 135–165 | 26–40 |
| AISI 1137 Annealed | 305–380 | 520–645 | 160–200 | 21–33 |
| AISI 1137 Normalized | 355–435 | 595–740 | 185–225 | 18–27 |
| AISI 1141 Annealed | 315–390 | 540–660 | 150–190 | 20–31 |
| AISI 1141 Normalized | 365–445 | 645–780 | 188–228 | 18–28 |
| AISI 1144 Annealed | 310–385 | 525–645 | 155–190 | 20–30 |
| AISI 1144 Normalized | 360–440 | 600–740 | 180–225 | 16–26 |
| AISI 1020 Annealed | 265–325 | 355–435 | 110–130 | 28–43 |
| AISI 1020 Normalized | 310–350 | 395–490 | 125–150 | 28–43 |
| AISI 1040 Annealed | 315–390 | 475–575 | 143–173 | 24–36 |
| AISI 1040 Normalized | 335–415 | 530–650 | 160–195 | 22–34 |
Resulfurized Steels Machinability: Machining Speed of AISI 1117, 1118, 12L14, 1137, 1141, 1144
| Grade | Annealed (m/min) | As rolled (m/min) | Normalized (m/min) |
|---|---|---|---|
| AISI 1117 | 45.7 | 42.7 | 45.7 |
| AISI 1118 | 45.7 | 42.7 | 45.7 |
| AISI 1137 | 36.6 | 33.5 | 30.5 |
| AISI 1141 | 36.6 | 30.5 | 29.9 |
| AISI 1144 | 45.7 | 36.6 | 36.6 |
| AISI 12L14 | — | 45.7 | — |
| AISI 1020 (reference) | 45.7 | 36.6 | 39.6 |
| AISI 1040 (reference) | 33.5 | 25.6 | 29.3 |
In the as rolled condition the highest machining speed in these data sheets belongs to AISI 12L14 (45.7 m/min). At a similar carbon level the resulfurized grades cut faster than their plain carbon counterparts: AISI 1117, 1118 and 12L14 are faster than plain AISI 1020, and AISI 1137, 1141 and 1144 are faster than plain AISI 1040. The trade-off is lower transverse ductility and poorer weldability, because the sulfide inclusions are elongated in the rolling direction; resulfurized grades are therefore not recommended for welded or heavily cold-formed parts.
Resulfurized Steels Strength Charts: As Rolled
Choosing Between Resulfurized Steels
Choose AISI 12L14 when machining speed and surface finish matter most and the part is lightly stressed. AISI 1117 and 1118 suit carburized or case-hardened parts that need a hard surface over a tough core. AISI 1137, 1141 and 1144 give higher strength in the as rolled or quenched and tempered condition for shafts, studs and spindles, while still machining easily. AISI 1117 | AISI 1118 | AISI 1137 | AISI 1141 | AISI 1144 | AISI 12L14
Looking for free-machining steel parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1117, 1144 and 12L14 parts in-house on automatic and CNC lathes, and inspects them before shipment.


4 Replies to “Resulfurized Free-Machining Steels Compared: AISI 1117, 1118, 12L14, 1137, 1141 and 1144 Composition, Properties and Machinability”
Comments are closed.