AISI 1117 Normalized Material Data Sheet

AISI 1117 Normalized Material Data Sheet

AISI 1117 Normalized Overview

AISI 1117 normalized is AISI 1117 resulfurized low carbon steel (UNS G11170) in the normalized condition. This AISI 1117 normalized material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1117 conditions in our AISI 1117 yield, tensile and hardness comparison. See also the resulfurized free-machining steels comparison. Looking for AISI 1117 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1117 steel parts in-house and inspects them before shipment.

AISI 1117 Normalized Designation

AISI 1117
ConditionNormalized
UNS numberG11170
US nameASTM G11170, ASTM 1117 Class A, ASTM 1117, AMS 5022
GB (Chinese) name~Y20
JIS (Japanese) nameSUM31L, SUM31

AISI 1117 Normalized Typical uses

Lightly stressed parts, e.g. camshafts, selector forks, ratchets, tappets

AISI 1117 Normalized Composition detail

C (carbon)0.14–0.2%
Fe (iron)98.3–98.8%
Mn (manganese)1–1.3%
P (phosphorus)0–0.04%
S (sulfur)0.08–0.13%

AISI 1117 Normalized Physical properties

Density7.8–7.9g/cm3

AISI 1117 Normalized Mechanical properties

Young’s modulus205–215GPa
Specific stiffness26.1–27.4MN.m/kg
Yield strength (elastic limit)270–335MPa
Tensile strength415–520MPa
Specific strength34.4–42.7kN.m/kg
Elongation26–40% strain
Compressive strength270–335MPa
Flexural modulus205–215GPa
Flexural strength (modulus of rupture)270–335MPa
Shear modulus79–84GPa
Bulk modulus158–175GPa
Poisson’s ratio0.285–0.295 
Shape factor61
Hardness – Vickers130–160HV
Elastic stored energy (springs)175–265kJ/m3
Fatigue strength at 10^7 cycles231–271MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
198–316MPa

AISI 1117 Normalized Impact & fracture properties

Fracture toughness48–78MPa.m0.5
Toughness (G)11.5–27.6kJ/m2

AISI 1117 Normalized Thermal properties

Melting point1490–1530°C
Maximum service temperature343–357°C
Minimum service temperature-63–-38°C
Thermal conductivity50–54W/m.°C
Specific heat capacity460–500J/kg.°C
Thermal expansion coefficient11.5–13µstrain/°C
Thermal shock resistance103–133°C
Thermal distortion resistance3.96–4.57MW/m
Latent heat of fusion270–275kJ/kg

AISI 1117 Normalized Electrical properties

Electrical resistivity15–20µohm.cm
Electrical conductivity8.62–11.5%IACS
Galvanic potential-0.52–-0.44V

AISI 1117 Normalized Magnetic properties

Magnetic typeMagnetic

AISI 1117 Normalized Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5110–5240m/s
Mechanical loss coefficient (tan delta)0.001–0.00126 

AISI 1117 Normalized Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingExcellent
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed45.7 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Poor
Carbon equivalency0.307 – 0.417

AISI 1117 Normalized Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

AISI 1117 Normalized Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Not susceptible

AISI 1117 Normalized Notes

AISI 1117 Normalized Warning
Free cutting’ steel – in common with all such steels, it is not recommended where welding is involved.
AISI 1117 Normalized Other notes
Designed for oil hardening, but can be water quenched for maximum case hardness.

AISI 1117 Normalized Standards with similar compositions

Canada: C1117 to CSA 94-1/1, CL.1.C1117 to CSA STAN95-1-1
India: A-N to IS 3945, B-N to IS 3945
Italy: CF17SMnPb10 to UNI 4838
Japan: SUM31 to JIS G4804, SUM31L to JIS G4804
Mexico: 1116 to NMX-B-301, 1117 to NMX-B-301
Pan America: 1117 to COPANT 330, 1117 to COPANT 331, 1117 to COPANT 333
UK: 15SMn13 to BS EN 10277-3, 170H15 to BS 970/1, 173H15 to BS 970/1, 173H16 to BS 970/1, 210A15 to BS 970/1, 210M15 to BS 970/1, 220M07 to BS 970/1
USA: 1114, 1116, 1116 to ASTM A29/A29M, 1117, 1117 Class A to ASTM A311/A311M, 1117 to ASTM A29/A29M, 1117 to ASTM A512-96, 1117 to MIL-S-18411, 1117 to SAE J403, 1120, 5022 to AMS 5022L, G11160 to ASTM A510/A510M, G11160 to ASTM A576-90b, G11170 to ASTM A510/A510M, G11170 to ASTM A576-90b, UNS G11160, UNS G11170, UNS K11711
Tradenames: AMERCUT C-1117, BRYMILL CH-2, DUNELT 5, JALCASE 6, LASALLE 1117, MARQUES D2SS, RYCASE, S-1117, YND-33