AISI 1118 Annealed vs As Rolled vs Normalized: Yield, Tensile & Hardness Compared

How do the AISI 1118 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength, hardness, elongation and machining speed of AISI 1118 resulfurized low carbon steel (UNS G11180) side by side for 3 conditions: annealed, as rolled, normalized. All values are taken from the individual AISI 1118 material data sheets linked below.

AISI 1118 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)Machining speed (m/min)
Annealed255–315405–495128–15027–4245.7
As Rolled285–350465–580143–17326–3842.7
Normalized285–355425–530135–16526–4045.7

AISI 1118 Differences Compared with Annealed

The table below shows how much each AISI 1118 condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength, hardness or elongation.

ConditionYield strengthTensile strengthHardnessElongation
As Rolled+11%+16%+14%-7%
Normalized+12%+6%+8%-4%

AISI 1118 Strength and Hardness Charts

AISI 1118 Yield strength by condition (MPa)Annealed255–315As Rolled285–350Normalized285–355
AISI 1118 Tensile strength by condition (MPa)Annealed405–495As Rolled465–580Normalized425–530
AISI 1118 Hardness by condition (HV)Annealed128–150As Rolled143–173Normalized135–165

AISI 1118 Heat Treatment Key Points

The highest tensile strength of AISI 1118 in these data sheets is reached in the as rolled condition (465–580 MPa). The softest condition is annealed (128–150 HV), with a machining speed of 45.7 m/min, which is usually preferred for machining and forming.

AISI 1118 is a resulfurized free-machining grade. See how it compares with the other free-machining steels in our resulfurized steels comparison.

AISI 1118 Material Data Sheets

AISI 1118 Annealed | AISI 1118 As Rolled | AISI 1118 Normalized | All AISI 1118 conditions

Looking for AISI 1118 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1118 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.