Home » Bronze Alloys » CuSn9Pb1 (C52400) Phosphor Bronze, Cast Material Data Sheet
CuSn9Pb1 (C52400) Phosphor Bronze, Cast Material Data Sheet
CuSn9Pb1 (C52400) Phosphor Bronze Material Data Sheet (Cast)
CuSn9Pb1 C52400 Cast Overview
CuSn9Pb1 C52400 cast is a cast bronze (UNS C52400), known as phosphor bronze. Condition: Cast. This CuSn9Pb1 C52400 cast material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C52400 bronze castings from Turkey (Türkiye)? Modulus Metal supplies C52400 bronze castings with in-house CNC machining and inspects them before shipment.
C52400 Designation
CuSn9Pb1
UNS number
C52400
C52400 Typical uses
Medium-duty gears, bearings and bushes.
CuSn9Pb1 C52400 Cast Composition detail
Cu (copper)
88.3
–
91
%
Fe (iron)
0
–
0.1
%
P (phosphorus)
0.03
–
0.35
%
Pb (lead)
0
–
0.05
%
Sn (tin)
9
–
11
%
Zn (zinc)
0
–
0.2
%
C52400 Physical properties
Density
8.8
–
8.82
g/cm3
CuSn9Pb1 C52400 Cast Mechanical properties
Young’s modulus
78
–
82
GPa
Specific stiffness
8.85
–
9.31
MN.m/kg
Yield strength (elastic limit)
140
–
230
MPa
Tensile strength
270
–
370
MPa
Specific strength
15.9
–
26.1
kN.m/kg
Elongation
2
–
10
% strain
Compressive strength
140
–
230
MPa
Flexural modulus
78
–
82
GPa
Flexural strength (modulus of rupture)
140
–
230
MPa
Shear modulus
28.9
–
30.3
GPa
Bulk modulus
84.2
–
88.6
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
26
Hardness – Vickers
95
–
140
HV
Elastic stored energy (springs)
129
–
315
kJ/m3
Fatigue strength at 10^7 cycles
137
–
168
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
111
–
207
MPa
C52400 Impact & fracture properties
Fracture toughness
50
–
65.5
MPa.m0.5
Toughness (G)
31.7
–
52.8
kJ/m2
CuSn9Pb1 C52400 Cast Thermal properties
Melting point
882
–
1040
°C
Maximum service temperature
150
–
170
°C
Minimum service temperature
-273
°C
Thermal conductivity
44
–
48
W/m.°C
Specific heat capacity
376
–
392
J/kg.°C
Thermal expansion coefficient
18
–
19
µstrain/°C
Thermal shock resistance
94.5
–
156
°C
Thermal distortion resistance
2.36
–
2.61
MW/m
Latent heat of fusion
220
–
240
kJ/kg
C52400 Electrical properties
Electrical resistivity
16.2
–
18.2
µohm.cm
Electrical conductivity
9.47
–
10.6
%IACS
Galvanic potential
-0.23
–
-0.15
V
C52400 Magnetic properties
Magnetic type
Non-magnetic
C52400 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2980
–
3050
m/s
Mechanical loss coefficient (tan delta)
7.6e-5
–
2.04e-4
C52400 Processing properties
Metal casting
Excellent
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
33.5 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Excellent
C52400 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuSn9Pb1 C52400 Cast Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible
C52400 Notes
CuSn9Pb1 C52400 Cast Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C52400 Standards with similar compositions
Tradenames: AMPCOLOY 711, BARR ALLOY NO. 15, BUNTING NO. 156, BUNTING NO. 907, C90700, FEDERAL-MOGUL F-20, HOLFOS CT1, HOLFOS PB3, HOLFOS W W, M H ALLOY NO. 15, MTEK 65, PHOSPHOR BRONZE NO. 3, SUPER-HOLFOS W.W, T-11-0-0, TAURUS BRONZE MARK II, TECHNI-CAST 1100, WRM 110