C93800 Leaded Bronze 76-9-15, Cast Material Data Sheet

C93800 Leaded Bronze 76-9-15 Material Data Sheet (Cast)

C93800 Cast Bronze Overview

C93800 cast bronze is a cast bronze (UNS C93800, EN CC496K), known as leaded bronze 76-9-15. Condition: Cast. This C93800 cast bronze material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C93800 bronze castings from Turkey (Türkiye)? Modulus Metal supplies C93800 bronze castings with in-house CNC machining and inspects them before shipment.

C93800 Designation

Copper Alloy: CuSn7Pb15 (UNS C93800)
UNS numberC93800
EN nameCC496K
ISO nameCuPb17Sn5
JIS (Japanese) nameLBC 4

C93800 Typical uses

Bearings and bushes to resist corrosion and poor lubrication (plasticity increases with lead content, making them suitable for minor misalignment and for use with soft steel shafts).

C93800 Cast Bronze Composition detail

Al (aluminum)0–0.005%
Cu (copper)73.6–80.7%
Fe (iron)0–0.15%
Ni (nickel)0–1%
P (phosphorus)0–0.05%
Pb (lead)13–16%
S (sulfur)0–0.08%
Sb (antimony)0–0.8%
Si (silicon)0–0.005%
Sn (tin)6.3–7.5%
Zn (zinc)0–0.8%

C93800 Physical properties

Density8.95–9g/cm3

C93800 Cast Bronze Mechanical properties

Young’s modulus70–72GPa
Specific stiffness7.8–8.02MN.m/kg
Yield strength (elastic limit)80–110MPa
Tensile strength170–230MPa
Specific strength8.91–12.3kN.m/kg
Elongation4–10% strain
Compressive strength80–110MPa
Flexural modulus70–72GPa
Flexural strength (modulus of rupture)80–110MPa
Shear modulus25.9–26.6GPa
Bulk modulus75.6–77.8GPa
Poisson’s ratio0.34–0.35 
Shape factor29
Hardness – Vickers50–70HV
Elastic stored energy (springs)46.1–83.4kJ/m3
Fatigue strength at 10^7 cycles101–123MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
82.9–150MPa

C93800 Impact & fracture properties

Fracture toughness73.1–82.6MPa.m0.5
Toughness (G)75.5–95.8kJ/m2

C93800 Cast Bronze Thermal properties

Melting point877–1020°C
Maximum service temperature180–190°C
Minimum service temperature-273  °C
Thermal conductivity50.2–54.4W/m.°C
Specific heat capacity376–392J/kg.°C
Thermal expansion coefficient18–19µstrain/°C
Thermal shock resistance60.8–84°C
Thermal distortion resistance2.69–2.97MW/m
Latent heat of fusion220–240kJ/kg

C93800 Electrical properties

Electrical resistivity14.8–15.4µohm.cm
Electrical conductivity11.2–11.6%IACS
Galvanic potential-0.28–-0.2V

C93800 Magnetic properties

Magnetic typeNon-magnetic

C93800 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2790–2830m/s
Mechanical loss coefficient (tan delta)3.31e-4–6.25e-4 

C93800 Processing properties

Metal castingExcellent
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed116 m/min
WeldabilityUnsuitable

C93800 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Contains lead which lubricates, improving resistance.
Excellent
FlammabilityNon-flammable

C93800 Cast Bronze Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible

C93800 Notes

C93800 Cast Bronze Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C93800 Standards with similar compositions

Japan: CAC604 to JIS H5120
USA: C93800, C93800 to ASTM B271, C93800 to ASTM B30, C93800 to ASTM B505, C93800 to ASTM B584, C93800 to ASTM B66, C93800 to ASTM B763, C93800 to CDA Datasheet, C93800 to MIL B-16261, C93800 to QQ C-390, C93800 to QQ C-525, C93800 to QQ L-225, C93800 to SAE J462, C93900 to ASTM B30, UNS C93800
Venezuela: C93800 to COPANT 801