CuSn6 (C51900) 7% Phosphor Bronze, Hard Material Data Sheet

CuSn6 (C51900) 7% Phosphor Bronze Material Data Sheet (Wrought, Hard)

CuSn6 C51900 Hard Overview

CuSn6 C51900 hard is a wrought bronze (UNS C51900, EN CW452K), known as 7% phosphor bronze. Condition: Hard. This CuSn6 C51900 hard material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C51900 bronze parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C51900 bronze parts in-house and inspects them before shipment.

C51900 Designation

CuSn6, wrought
ConditionHard
UNS numberC51900
EN nameCW452K
ISO nameCuSn6
GB (Chinese) nameQSn6.5-0.1 / QSn6.5-0.4 / QSn7-0.2
JIS (Japanese) nameC5191

C51900 Typical uses

Springs, clips, fixings, washers, anti-friction components, wire brushes, pinions and gears, pump parts, welding rods & electrodes, tubes to resist corrosion & erosion.

CuSn6 C51900 Hard Composition detail

Cu (copper)92.2–95%
Fe (iron)0–0.1%
P (phosphorus)0.03–0.35%
Pb (lead)0–0.05%
Sn (tin)5–7%
Zn (zinc)0–0.3%

C51900 Physical properties

Density8.6–8.62g/cm3

CuSn6 C51900 Hard Mechanical properties

Young’s modulus112–115GPa
Specific stiffness13–13.4MN.m/kg
Yield strength (elastic limit)560–570MPa
Tensile strength640–650MPa
Specific strength65–66.2kN.m/kg
Elongation13–14% strain
Compressive strength560–570MPa
Flexural modulus112–115GPa
Flexural strength (modulus of rupture)560–570MPa
Shear modulus41.4–42.6GPa
Bulk modulus121–124GPa
Poisson’s ratio0.34–0.35 
Shape factor17
Hardness – Vickers200–210HV
Elastic stored energy (springs)1380–1440kJ/m3
Fatigue strength at 10^7 cycles240–242MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
237–245MPa

C51900 Impact & fracture properties

Fracture toughness26.4–26.8MPa.m0.5
Toughness (G)6.11–6.36kJ/m2

CuSn6 C51900 Hard Thermal properties

Melting point922–1050°C
Maximum service temperature160–170°C
Minimum service temperature-273  °C
Thermal conductivity66–68W/m.°C
Specific heat capacity384  J/kg.°C
Thermal expansion coefficient16.5–17.5µstrain/°C
Thermal shock resistance283–303°C
Thermal distortion resistance3.81–4.07MW/m
Latent heat of fusion220–240kJ/kg

C51900 Electrical properties

Electrical resistivity14.8–16.6µohm.cm
Electrical conductivity10.4–11.6%IACS
Temperature dependence of resistivity2–2.5/°C
Galvanic potential-0.22–-0.14V

C51900 Magnetic properties

Magnetic typeNon-magnetic

C51900 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3610–3650m/s
Mechanical loss coefficient (tan delta)1.2e-5–1.3e-5 

C51900 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingUnsuitable
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed33.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good

C51900 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuSn6 C51900 Hard Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible

C51900 Notes

CuSn6 C51900 Hard Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C51900 Standards with similar compositions

Czech Republic: CuSn6 to CSN 423016
Denmark: 5428 to DS 3003
Europe: CW452K to CEN EN 12163, CW452K to CEN EN 12166, CW452K to CEN EN 12167, CW452K to CEN EN 12449, CW452K to CEN EN 1652, CW452K to CEN EN 1654
Germany: 2.102 to DIN, CuSn6 to DIN, SnBz6 to DIN
Sweden: 5428-02 to SIS 145428, 5428-04 to SIS 145428, 5428-05 to SIS 145428
UK: C11 to BS 2901/3
USA: C51900, UNS C51900
Tradenames: 5190, BOLTON NO. 11 PHOSPHOR BRONZE, ELEPHANT BRAND NO. 175 METAL, HAIRSPRINGS, LNT CUSN 6, PHOSPHOR BRONZE 320, PHOSPHOR BRONZE HAIRSPRINGS, PHOSPHOR BRONZE, RUSSIAN, PHOSPHORBRONZE SN BZ 6, SEYMOUR 9231, ZINNBRONZE SNBZ6