Home » Bronze Alloys » CuSn6 (C51900) 7% Phosphor Bronze, Extra Hard Material Data Sheet
CuSn6 (C51900) 7% Phosphor Bronze, Extra Hard Material Data Sheet
CuSn6 (C51900) 7% Phosphor Bronze Material Data Sheet (Wrought, Extra Hard)
CuSn6 C51900 Extra Hard Overview
CuSn6 C51900 extra hard is a wrought bronze (UNS C51900, EN CW452K), known as 7% phosphor bronze. Condition: Extra hard. This CuSn6 C51900 extra hard material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C51900 bronze parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C51900 bronze parts in-house and inspects them before shipment.
C51900 Designation
CuSn6, wrought
Condition
Extra hard
UNS number
C51900
EN name
CW452K
ISO name
CuSn6
GB (Chinese) name
QSn6.5-0.1 / QSn6.5-0.4 / QSn7-0.2
JIS (Japanese) name
C5191
C51900 Typical uses
Springs, clips, fixings, washers, anti-friction components, wire brushes, pinions and gears, pump parts, welding rods & electrodes, tubes to resist corrosion & erosion.
CuSn6 C51900 Extra Hard Composition detail
Cu (copper)
92.2
–
95
%
Fe (iron)
0
–
0.1
%
P (phosphorus)
0.03
–
0.35
%
Pb (lead)
0
–
0.05
%
Sn (tin)
5
–
7
%
Zn (zinc)
0
–
0.3
%
C51900 Physical properties
Density
8.6
–
8.62
g/cm3
CuSn6 C51900 Extra Hard Mechanical properties
Young’s modulus
112
–
115
GPa
Specific stiffness
13
–
13.4
MN.m/kg
Yield strength (elastic limit)
620
–
650
MPa
Tensile strength
700
–
720
MPa
Specific strength
72
–
75.5
kN.m/kg
Elongation
7
–
8
% strain
Compressive strength
620
–
650
MPa
Flexural modulus
112
–
115
GPa
Flexural strength (modulus of rupture)
620
–
650
MPa
Shear modulus
41.4
–
42.6
GPa
Bulk modulus
121
–
124
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
15
Hardness – Vickers
210
–
220
HV
Elastic stored energy (springs)
1690
–
1860
kJ/m3
Fatigue strength at 10^7 cycles
254
–
259
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
249
–
264
MPa
C51900 Impact & fracture properties
Fracture toughness
23.8
–
24.7
MPa.m0.5
Toughness (G)
4.98
–
5.39
kJ/m2
CuSn6 C51900 Extra Hard Thermal properties
Melting point
922
–
1050
°C
Maximum service temperature
160
–
170
°C
Minimum service temperature
-273
°C
Thermal conductivity
66
–
68
W/m.°C
Specific heat capacity
384
J/kg.°C
Thermal expansion coefficient
16.5
–
17.5
µstrain/°C
Thermal shock resistance
316
–
343
°C
Thermal distortion resistance
3.81
–
4.07
MW/m
Latent heat of fusion
220
–
240
kJ/kg
C51900 Electrical properties
Electrical resistivity
16.2
–
18.2
µohm.cm
Electrical conductivity
9.47
–
10.6
%IACS
Temperature dependence of resistivity
2
–
2.5
/°C
Galvanic potential
-0.22
–
-0.14
V
C51900 Magnetic properties
Magnetic type
Non-magnetic
C51900 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3610
–
3650
m/s
Mechanical loss coefficient (tan delta)
9e-6
–
1e-5
C51900 Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Unsuitable
Metal press forming
Acceptable
Metal deep drawing
Limited use
Machining speed
33.5 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
C51900 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuSn6 C51900 Extra Hard Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible
C51900 Notes
CuSn6 C51900 Extra Hard Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C51900 Standards with similar compositions
Czech Republic: CuSn6 to CSN 423016
Denmark: 5428 to DS 3003
Europe: CW452K to CEN EN 12163, CW452K to CEN EN 12166, CW452K to CEN EN 12167, CW452K to CEN EN 12449, CW452K to CEN EN 1652, CW452K to CEN EN 1654
Germany: 2.102 to DIN, CuSn6 to DIN, SnBz6 to DIN
Sweden: 5428-02 to SIS 145428, 5428-04 to SIS 145428, 5428-05 to SIS 145428