CuSn4 (C50900) 3% Phosphor Bronze, Soft Material Data Sheet

CuSn4 (C50900) 3% Phosphor Bronze Material Data Sheet (Wrought, Soft)

CuSn4 C50900 Soft Overview

CuSn4 C50900 soft is a wrought bronze (UNS C50900, EN CW450K), known as 3% phosphor bronze. Condition: Soft. This CuSn4 C50900 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C50900 bronze parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C50900 bronze parts in-house and inspects them before shipment.

C50900 Designation

CuSn4, wrought
ConditionSoft
UNS numberC50900
EN nameCW450K
ISO nameCuSn4
GB (Chinese) nameQSn4-0.3
JIS (Japanese) nameC5111

C50900 Typical uses

Tube plates for condensers & pressure vessels, bellows & diaphragms, masonry fixings, screws, bolts, rivets, washers, springs, clips, electrical contacts, switch parts, instrument components.

CuSn4 C50900 Soft Composition detail

Cu (copper)95.4–97.5%
Fe (iron)0–0.1%
P (phosphorus)0.03–0.3%
Pb (lead)0–0.05%
Sn (tin)2.5–3.8%
Zn (zinc)0–0.3%

C50900 Physical properties

Density8.83–8.85g/cm3

CuSn4 C50900 Soft Mechanical properties

Young’s modulus118–122GPa
Specific stiffness13.3–13.8MN.m/kg
Yield strength (elastic limit)100–110MPa
Tensile strength310–320MPa
Specific strength11.3–12.4kN.m/kg
Elongation54–55% strain
Compressive strength100–110MPa
Flexural modulus118–122GPa
Flexural strength (modulus of rupture)100–110MPa
Shear modulus43.7–45.1GPa
Bulk modulus127–132GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers70–75HV
Hardness – Brinell63–67HB
Elastic stored energy (springs)41.7–50.4kJ/m3
Fatigue strength at 10^7 cycles150–153MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
147–157MPa

C50900 Impact & fracture properties

Fracture toughness73.1–76MPa.m0.5
Toughness (G)44.4–48.3kJ/m2

CuSn4 C50900 Soft Thermal properties

Melting point947–1070°C
Maximum service temperature150–160°C
Minimum service temperature-273  °C
Thermal conductivity84–86W/m.°C
Specific heat capacity385  J/kg.°C
Thermal expansion coefficient16.5–17.5µstrain/°C
Thermal shock resistance48.5–54.5°C
Thermal distortion resistance4.85–5.16MW/m
Latent heat of fusion220–240kJ/kg

C50900 Electrical properties

Electrical resistivity11.3–11.7µohm.cm
Electrical conductivity14.7–15.3%IACS
Temperature dependence of resistivity2–2.5/°C
Galvanic potential-0.21–-0.13V

C50900 Magnetic properties

Magnetic typeNon-magnetic

C50900 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3650–3720m/s
Mechanical loss coefficient (tan delta)3.31e-4–4e-4 

C50900 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingLimited use
Metal press formingExcellent
Metal deep drawingAcceptable
Machining speed33.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good

C50900 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuSn4 C50900 Soft Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible

C50900 Notes

CuSn4 C50900 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C50900 Standards with similar compositions

UK: PB101 to BS 2870, PB101 to BS 2875
USA: C50900, UNS C50800, UNS C50900
Tradenames: BOLTON NO. 12 PHOSPHOR BRONZE, BRONZE, PHOSPHOR GRADE A, ELEPHANT BRAND NO. 3 METAL, HI-10, M.S. BRONZE, PHOSPHOR BRONZE 301, RIVERSIDE GRADE E PHOSPHOR BRONZE, SEYMOUR 9370, SEYMOUR 971, SEYMOUR 9971, SUPER X PHOSPHOR BRONZE GR. E ALLOY 101