C94100 Leaded Bronze 75-5-20, Cast Material Data Sheet

C94100 Leaded Bronze 75-5-20 Material Data Sheet (Cast)

C94100 Cast Bronze Overview

C94100 cast bronze is a cast bronze (UNS C94100, EN CC497K), known as leaded bronze 75-5-20. Condition: Cast. This C94100 cast bronze material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C94100 bronze castings from Turkey (Türkiye)? Modulus Metal supplies C94100 bronze castings with in-house CNC machining and inspects them before shipment.

C94100 Designation

Copper Alloy: CuSn5Pb20 (UNS C94100)
UNS numberC94100
EN nameCC497K
ISO nameCuPb20Sn5
GB (Chinese) nameCuPb20Sn5

C94100 Typical uses

Steel-backed bearings for car and aero engines.

C94100 Cast Bronze Composition detail

Al (aluminum)0–0.005%
Cu (copper)68.3–77.5%
Fe (iron)0–0.25%
Ni (nickel)0–1%
P (phosphorus)0–0.05%
Pb (lead)18–22%
S (sulfur)0–0.08%
Sb (antimony)0–0.8%
Si (silicon)0–0.005%
Sn (tin)4.5–6.5%
Zn (zinc)0–1%

C94100 Physical properties

Density8.95–9.05g/cm3

C94100 Cast Bronze Mechanical properties

Young’s modulus68–72GPa
Specific stiffness7.55–8MN.m/kg
Yield strength (elastic limit)60–100MPa
Tensile strength160–190MPa
Specific strength6.67–11.1kN.m/kg
Elongation5–10% strain
Compressive strength60–100MPa
Flexural modulus68–72GPa
Flexural strength (modulus of rupture)60–100MPa
Shear modulus25.2–26.6GPa
Bulk modulus73.4–77.8GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers45–65HV
Elastic stored energy (springs)27.1–67.9kJ/m3
Fatigue strength at 10^7 cycles97–109MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
86.3–123MPa

C94100 Impact & fracture properties

Fracture toughness76–90.5MPa.m0.5
Toughness (G)83–116kJ/m2

C94100 Cast Bronze Thermal properties

Melting point927–1060°C
Maximum service temperature180–190°C
Minimum service temperature-273  °C
Thermal conductivity70–76W/m.°C
Specific heat capacity376–392J/kg.°C
Thermal expansion coefficient18–19µstrain/°C
Thermal shock resistance46.3–77.4°C
Thermal distortion resistance3.76–4.14MW/m
Latent heat of fusion220–240kJ/kg

C94100 Electrical properties

Electrical resistivity11.7–12.9µohm.cm
Electrical conductivity13.4–14.7%IACS
Galvanic potential-0.28–-0.2V

C94100 Magnetic properties

Magnetic typeNon-magnetic

C94100 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2750–2830m/s
Mechanical loss coefficient (tan delta)4e-4–0.00111 

C94100 Processing properties

Metal castingExcellent
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed122 m/min
WeldabilityUnsuitable

C94100 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Contains lead which lubricates, improving resistance.
Excellent
FlammabilityNon-flammable

C94100 Cast Bronze Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible

C94100 Notes

C94100 Cast Bronze Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C94100 Standards with similar compositions

Australia: C94100 to AS 2738
USA: C94100, C94100 to ASTM B505, C94100 to ASTM B67, C94100 to CDA Datasheet, C94500, UNS C94100, UNS C94500
Tradenames: BUNTING BEARINGS M 40, WRM 619